Lead smelting water-quenched slag-based cementitious material, and preparation method and application thereof

Through the combination of mechanical ball milling and alkali excitation, and the use of microwave irradiation technology, the problems of low dosage, long curing time and low strength of lead smelting water quenching slag in cementitious materials have been solved, and the compressive strength of highly efficient preparation can reach 78.1 MPa lead smelting water quenching slag-based cementitious material, suitable for construction projects.

CN116375430BActive Publication Date: 2024-10-15CENT SOUTH UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310472770.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-10-15
Estimated Expiration
2043-04-27

AI Technical Summary

Technical Problem

The problems of lead smelting water quenching slag in cementitious materials include low content, long curing time and low strength.

Method used

Mechanical ball milling is used to improve the particle size distribution and chemical activity of lead smelting water quenching slag, and it is activated by alkali activators and combined with microwave irradiation technology to shorten the curing time and improve the compressive strength.

Benefits of technology

Significantly improve the compressive strength of lead smelting water quenching slag-based cementitious material, shorten the curing time from 28 days to 3 minutes, and reduce the leaching rate of heavy metals and harmful substances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116375430B_ABST
    Figure CN116375430B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a lead smelting water-quenched slag-based cementitious material based on microwave curing, comprising the steps of: S1, activating and modifying the lead smelting water-quenched slag to obtain a pretreated material; S2, mixing the pretreated material, an alkali activator and water to obtain a slurry; S3, curing the slurry to obtain a cured product; S4, subjecting the cured product to microwave treatment to obtain a lead smelting water-quenched slag-based cementitious material; the microwave power of the microwave treatment is 560-700w, and the irradiation time of the microwave treatment is 1-3min. The present invention prepares a lead smelting water-quenched slag-based cementitious material with high compressive strength, which can be used in the fields of house construction, road construction, etc.; compared with the existing water-quenched slag-based cementitious material, not only the curing time is shortened from 28 days to within 3 minutes, but also the compressive strength is significantly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of green cementitious material preparation, and in particular to a lead smelting water-quenched slag-based cementitious material, and a preparation method and application thereof. Background Art

[0002] Lead smelting water-quenched slag (hereinafter referred to as "lead slag") is a product of high-temperature molten slag after water quenching and cooling. It contains certain silicon and aluminum components and amorphous glass phase and has potential cementing activity. At present, the use of lead smelting water-quenched slag to prepare cementitious materials mainly includes partial replacement of iron raw materials for making cement clinker, preparation of concrete or cement-based cementitious materials as admixtures, and direct preparation of alkali-activated lead slag-based cementitious materials.

[0003] Metallurgical waste slag treated with water quenching has potential gelling activity, and the research on its application in building materials is very mature. In "Research on the Preparation of Composite Cement with Large Amounts of Coal Slag and Manganese Slag", Chen Xiangrong et al. used water-quenched manganese slag to prepare composite cement. When the amount of coal slag was 30% and the amount of manganese slag was 20%, qualified PC32.5 cement could be prepared. In the Chinese invention patent with application number 202111116565, blast furnace water-quenched slag, steel slag, and casting slag were mixed and ground to prepare alkali-activated cementitious materials. The strength can reach 34.5MPa after standard curing for 28 days. Water-quenched slag-based cementitious materials are also often used as adhesives for mine filling materials. In "Preparation and Performance of New Cementitious Materials for Lead-Zinc Tailings", Liu Long et al. ground blast furnace water-quenched slag with alkali activators, and the prepared new cementitious materials were mixed with lead-zinc tailings. When the amount was half of PC42.5 cement, higher strength could be achieved. In the Chinese invention patent with application number 202011456289, copper smelting water-quenched slag powder is mixed with steel slag powder, cement clinker, gypsum and other auxiliary agents and ground into a new type of cementitious material. When the copper smelting water-quenched slag is added at 32%, the strength after 28 days of curing can reach 7.08MPa.

[0004] Lead smelting water-quenched slag has high iron content, low alkaline content, and low activity, making it difficult to use in large quantities for cement production. Therefore, how to improve the activity of lead slag and increase its incorporation into building materials has become a hot research topic in recent years. The more traditional method is to use mechanical activation to grind the lead slag to stimulate its chemical activity, and add chemical activators such as silicate cement, calcium sulfate, and water glass to produce a cementitious material with a certain strength. For example, in the Chinese invention patent with application number 202210313751, the lead smelting water-quenched slag is first ground using a ball mill / vertical mill, and then a certain proportion of calcium-based, magnesium-based materials and silicate cement are added. After high-temperature steam curing for 1 day and conventional curing for 28 days, a cementitious material with a strength of 50MPa can be obtained.

[0005] In the above-mentioned applications, there are still many areas that need improvement: (1) The water-quenched slag is not fully activated, and its content in cementitious materials is low (20-40%), and it requires the assistance of a large amount of highly active raw materials such as cement clinker and blast furnace slag; (2) The curing time is long, and it often takes more than 28 days of curing to achieve a high mechanical strength; (3) Except for a few studies, the strength of the prepared cementitious materials is relatively low, and if a high mechanical strength is to be obtained, it usually requires a period of high-temperature curing (steam curing) to solubilize and reconstruct the raw materials to shorten the curing time and improve the mechanical strength. Even if a certain high-temperature treatment is applied in the early stage of curing, a longer curing time (28-32 days) is still required to ensure the later strength and stability.

[0006] In view of this, it is necessary to provide a lead smelting water-quenched slag-based cementitious material, and a preparation method and application thereof, so as to solve or at least alleviate the above-mentioned technical defects of low water-quenched slag dosage, long curing time and low strength. Summary of the invention

[0007] The main purpose of the present invention is to provide a lead smelting water-quenched slag-based cementitious material, and a preparation method and application thereof, aiming to solve or at least alleviate the above-mentioned technical problems of low water-quenched slag dosage, long curing time and low strength.

[0008] To achieve the above object, the present invention provides a method for preparing a lead smelting water-quenched slag-based cementitious material based on microwave curing, comprising the steps of:

[0009] S1, subjecting the lead smelting water-quenched slag to an activation modification treatment to obtain a pre-treated product; wherein the activation modification treatment comprises: ball milling the lead smelting water-quenched slag;

[0010] S2, mixing the pretreated material, an alkali activator and water to obtain a slurry; wherein the water glass modulus of the alkali activator is 1-1.5;

[0011] The mass ratio of the pretreatment material to the alkaline activator is 88-95:5-12;

[0012] The water: the sum of the pre-treated material and the alkaline activator is 0.15-0.25 ml: 1 g;

[0013] S3, curing the slurry to obtain a cured product;

[0014] S4, subjecting the solidified product to microwave treatment to obtain a lead smelting water-quenched slag-based gelling material; wherein the microwave power of the microwave treatment is 560-700w, and the irradiation time of the microwave treatment is 1-3min.

[0015] Furthermore, the lead smelting water-quenched slag contains iron elements, and the mass proportion of the iron elements in the lead smelting water-quenched slag is 25-30%.

[0016] Furthermore, the activation modification treatment further comprises: before the ball milling, grinding the lead smelting water-quenched slag;

[0017] The ground lead smelting water-quenched slag is passed through a 20-50 mesh sieve, and the sieve residue is subjected to ball milling.

[0018] Furthermore, the grinding is carried out in a vibration mill, and the vibration grinding time of the lead smelting water-quenched slag in the vibration mill is 30-120s.

[0019] Furthermore, the activation modification treatment further comprises: passing the ball-milled product through a 100-200 mesh sieve, and taking the sieve-under material as the pretreated product.

[0020] Furthermore, in the ball milling, the ball milling speed is 250-350 r / min, the ball-to-material mass ratio is 4-12:1, and the ball milling time is 30-60 min.

[0021] Furthermore, the curing treatment includes: curing and molding the slurry in a mold to obtain a cured product.

[0022] Furthermore, the microwave frequency of the microwave treatment is 2450 MHz.

[0023] The present invention also provides a lead smelting water-quenched slag-based gelling material, which is prepared by any one of the preparation methods described above.

[0024] The present invention also provides a use of the lead smelting water-quenched slag-based cementitious material as described in any one of the above items in construction engineering.

[0025] Compared with the prior art, the present invention has at least the following advantages:

[0026] The present invention effectively improves the particle size distribution and chemical activity of lead smelting water-quenched slag through mechanical ball milling, and uses an alkali activator to further activate the volcanic ash activity of lead smelting water-quenched slag; in addition, the present invention effectively shortens the curing time of the cementitious material by using microwave irradiation, shortening the curing process that originally required 28 days to within 3 minutes, and the compressive strength is also significantly improved.

[0027] The preparation process of the present invention is simple to operate, the raw materials are easily available, the production discharge is less, the leaching rate of heavy metals and other harmful substances in the product is low, and it has considerable mechanical strength; based on the improvement of the preparation method, the cementitious material provided by the present invention can effectively serve as a variety of building materials and has practical value. That is, the present invention quickly prepares a water-quenched slag-based cementitious material with a compressive strength of up to 78.1 MPa through the combination of mechanical activation, alkali excitation, and microwave irradiation, which can be used in construction engineering fields such as house construction and road construction. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0029] Figure 1 is the XRD diagram of the lead smelting water-quenched slag in the present invention;

[0030] Figure 2 This is a data comparison chart of the compressive strength of lead smelting water-quenched slag-based cementitious materials under 700W microwave power and different irradiation durations in the present invention;

[0031] Figure 3 This is a data comparison chart of the compressive strength of lead smelting water-quenched slag-based cementitious materials under 2 minutes of irradiation time and different microwave powers in the present invention;

[0032] Figure 4 This is a physical picture of the slurry in Example 1;

[0033] Figure 5 This is a physical picture of the cured product in Example 1;

[0034] Figure 6 This is a physical picture of the lead smelting water-quenched slag-based cementitious material in Example 1;

[0035] Figure 7 This is a physical picture of the PO 42.5 block treated with microwaves in Comparative Example 7.

[0036] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0039] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention are familiar to those skilled in the art and the description of the present invention, and any methods, equipment and materials of the prior art similar or equivalent to the methods, equipment and materials described in the embodiments of the present invention can also be used to implement the present invention.

[0040] The present invention provides a method for preparing a lead smelting water-quenched slag-based cementitious material based on microwave curing. The lead smelting water-quenched slag-based cementitious material can also be understood as an application process of lead smelting water-quenched slag in cementitious materials.

[0041] It should be noted that, in a general sense, a cementitious material refers to a substance that can be transformed from a slurry into a solid stone-like body under physical and chemical effects, and can be cemented with other materials to form a composite solid with a certain mechanical strength. For the sake of ease of description, the present invention directly refers to the product after solidification and curing (microwave) as a lead smelting water-quenched slag-based cementitious material, but it does not affect the understanding of the cementitious process of the present invention by those skilled in the art. In the process of obtaining the lead smelting water-quenched slag-based cementitious material, those skilled in the art can also cement other materials to enhance the applicability of the present invention.

[0042] The preparation method of the lead smelting water-quenched slag-based gelling material comprises the following steps:

[0043] S1, subjecting lead smelting water-quenched slag to an activation and modification treatment to obtain a pretreated product; the pretreated product is the lead smelting water-quenched slag after the activation and modification treatment.

[0044] It should be understood that the lead smelting water-quenched slag used in the present invention is produced by water quenching in the lead smelting fuming furnace process, and the lead smelting water-quenched slag contains iron, and the mass proportion of the iron element in the lead smelting water-quenched slag is 25-30%. It should also be understood that the lead smelting water-quenched slag usually contains compounds of elements such as Ca, Si, and Al, which have potential gelling activity.

[0045] The activation modification treatment comprises: ball milling the lead smelting water-quenched slag; in the ball milling, the ball milling speed is 250-350r / min, the ball-to-material mass ratio is 4-12:1, and the ball milling time is 30-60min.

[0046] The activation modification treatment may further include: grinding the lead smelting water-quenched slag before the ball milling; the grinding may be performed in a vibration mill, and the vibration (grinding) time of the lead smelting water-quenched slag in the vibration mill may be 30-120s.

[0047] After the grinding, the lead smelting water-quenched slag that has been subjected to the grinding treatment can be passed through a 20-50 mesh sieve, and the sieve underflow can be taken for the ball milling.

[0048] The activation modification treatment may further include: passing the ball-milled product through a 100-200 mesh sieve, and taking the sieve residue as the pre-treated product.

[0049] S2, mixing the pretreated material, an alkali activator and water to obtain a slurry.

[0050] The preparation components of the alkali activator may include or be water glass and sodium hydroxide. After the preparation is completed, the water glass modulus of the alkali activator is 1-1.5, preferably, the water glass modulus of the alkali activator may be 1.1-1.2; wherein the original modulus of the water glass used in the alkali activator may be 3.0-3.3; the mass ratio of the pretreated material to the alkali activator is 88-95:5-12.

[0051] The water: the sum of the pretreated material and the alkaline activator is 0.15-0.25 ml: 1 g, preferably 0.2 ml: 1 g; by determining this ratio, the pretreated material and the alkaline activator can be adjusted into a slurry with a suitable water-cement ratio.

[0052] S3, curing the slurry to obtain a cured product.

[0053] The curing process may include: curing the slurry in a mold to obtain a cured product; the curing process is mainly to cure the slurry. The curing time may be 12-24 hours, and the curing method may be: standing curing at a temperature of 25°C and a relative humidity of 95%.

[0054] S4, after demolding the solidified product, subjecting the solidified product to microwave treatment to obtain a lead smelting water-quenched slag-based gelling material; the lead smelting water-quenched slag-based gelling material is a product of gelling the lead smelting water-quenched slag, and has high mechanical strength and chemical stability.

[0055] Wherein, the microwave power of the microwave treatment is 560-700w, and the irradiation time of the microwave treatment is 1-3min; preferably, the microwave power may be 600-700w or 650-700w, and the irradiation time may be 2-3min; the microwave frequency of the microwave treatment is 2450MHz.

[0056] The present invention adopts a mechanical ball milling method to activate and modify the lead smelting water-quenched slag, and the obtained modified lead smelting water-quenched slag is excited by water glass and then continuously cured to obtain the lead smelting water-quenched slag-based alkali-activated gelling material, and the obtained smelting water-quenched slag-based alkali-activated gelling material is subjected to microwave curing to obtain the microwave-assisted lead smelting water-quenched slag-based high-strength gelling material.

[0057] The present invention reduces the negative influence of the Fe-containing components in the water-quenched slag on the hydration process by microwave irradiation, and takes advantage of its high efficiency in absorbing microwaves, thereby greatly reducing the curing time and improving the mechanical strength of the cementitious material.

[0058] That is, the present invention applies microwave-assisted means on the basis of mechanical activation-alkali excitation activation, shortens the processing time to within 3 minutes, and can ensure high mechanical strength and chemical stability.

[0059] Since the lead smelting water-quenched slag-based cementitious material not only has relatively excellent performance, but also has specific components (consisting of lead smelting water-quenched slag, alkali activator and water) and almost 100% lead smelting water-quenched slag dosage (except alkali activator and water, all are lead smelting water-quenched slag); the present invention also provides a lead smelting water-quenched slag-based cementitious material, which is prepared by any of the preparation methods described above.

[0060] Since the lead smelting water-quenched slag-based cementitious material has high strength and extremely short curing time, the present invention also provides a use of the lead smelting water-quenched slag-based cementitious material as described in any one of the above items in a construction project.

[0061] The following are specific examples of the present invention:

[0062] Comparative Example 1

[0063] The preparation of lead smelting water quenching slag based cementitious material comprises the following steps:

[0064] 1. Take a dry lead smelting water-quenched slag sample and grind it with a vibration mill (vibration mill for 60 seconds), and pass it through a 50-mesh sieve; then take the sieved sample (screen under) and put it into a ball mill, control the ball mill speed to 250r / min, the material ball mass ratio to 8:1, the ball milling time to 30min, pass it through a 200-mesh sieve after ball milling, and take the screen under as the modified lead smelting water-quenched slag.

[0065] The main chemical components of the lead smelting water quenching slag used in this comparative example are as follows:

[0066] element Fe Ca Al Mg Si Pb As Cd Zn Content (wt%) 26.9 12.7 4.62 1.28 14.49 0.004 0.0004 <0.0001 0.029

[0067] The leaching toxicity of the lead smelting water quenching slag used in this comparative example is as follows:

[0068] element As Cd Cr Cu Ni Pb Zn Leaching toxicity (mg / L) 0.03 ND ND 0.01 ND 0.02 0.03 GB standard (mg / L) <5 <1 <5 <100 <5 <5 <100

[0069] Note: ND means below detection limit

[0070] In addition, refer to Figure 1 As shown, the lead smelting water-quenched slag used in this comparative example is mainly composed of amorphous glass and has good reactivity.

[0071] 2. Weigh 109.2 g of modified lead smelting water-quenched slag; prepare an alkaline activator with 8.7 g of water glass stock solution (original water content 58 wt%, modulus 3.0-3.3, derived from the ingredient table of the reagent) and 2.4 g of sodium hydroxide solid (the modulus of the activator is 1.1-1.2 at this time), mix the prepared alkaline activator with water, add it to the modified lead smelting water-quenched slag weighed above and mix it evenly to obtain a slurry; wherein, the water-ash mass ratio needs to be controlled to be 0.2 ml / g, and the mass of the ash refers to the sum of the masses of the modified lead smelting water-quenched slag and the alkaline activator.

[0072] 3. Inject the slurry into 2×2×2cm 3 The mold is placed in a mold, cured (cured) for 1 day at a temperature of 25° C. and a relative humidity of 95%, and then demolded to obtain a cured product.

[0073] 4. The solidified product after demoulding was continuously cured for 28 days under the above conditions (temperature of 25° C. and relative humidity of 95%) to obtain a lead smelting water-quenched slag-based cementitious material; its infinite side compressive strength was measured to be 50.7 MPa.

[0074] Example 1

[0075] Compared with Comparative Example 1, in this embodiment, only the curing 28d in step 4 is adjusted to microwave treatment of the cured product after demolding, and other conditions remain unchanged.

[0076] The microwave treatment was carried out in a microwave oven (2450 MHz), the microwave power was controlled to be 700 W, and the irradiation time was 1 min.

[0077] In this embodiment, after microwave treatment, a lead smelting water-quenched slag-based cementitious material is obtained; its infinite side compressive strength is measured to be 57.2 MPa, specifically corresponding to Figure 2 Compressive strength at 1 min irradiation time (abscissa).

[0078] In this embodiment, the appearance of the slurry is as follows Figure 4 The appearance of the cured product is as shown in Figure 5 As shown in the figure, the appearance of the lead smelting water-quenched slag-based alkali-activated cementitious material is as follows Figure 6 As shown; it can be seen that the present invention realizes the gelling and solidification of lead smelting water-quenched slag from slurry to solidified product, and completes the microwave irradiation of the solidified product.

[0079] Example 2

[0080] Compared with Example 1, in this example, only the irradiation time is adjusted to 1.5 min, and other conditions remain unchanged.

[0081] In this embodiment, after microwave treatment, a lead smelting water-quenched slag-based cementitious material is obtained; its infinite side compressive strength is measured to be 61.9 MPa, specifically corresponding to Figure 2 Compressive strength at 1.5 min irradiation time (abscissa).

[0082] Example 3

[0083] Compared with Example 1, in this example, only the irradiation time is adjusted to 2 minutes, and other conditions remain unchanged.

[0084] In this embodiment, after microwave treatment, a lead smelting water-quenched slag-based cementitious material is obtained; its infinite side compressive strength is measured to be 66.2 MPa, specifically corresponding to Figure 2 The compressive strength of the 2-min irradiation time (horizontal axis) and the corresponding Figure 3 Compressive strength at 700W microwave power (abscissa).

[0085] Example 4

[0086] Compared with Example 1, in this example, only the irradiation time is adjusted to 2.5 min, and other conditions remain unchanged.

[0087] In this embodiment, after microwave treatment, a lead smelting water-quenched slag-based cementitious material is obtained; its infinite side compressive strength is measured to be 78.1 MPa, specifically corresponding to Figure 2 Compressive strength at 2.5 min irradiation time (abscissa).

[0088] Example 5

[0089] Compared with Example 1, in this example, only the irradiation time is adjusted to 3 minutes, and other conditions remain unchanged.

[0090] In this embodiment, after microwave treatment, a lead smelting water-quenched slag-based cementitious material is obtained; its infinite side compressive strength is measured to be 73.1 MPa, specifically corresponding to Figure 2 Compressive strength at 3 min irradiation time (abscissa).

[0091] Comparative Example 2

[0092] Compared with Example 1, in this comparative example, only the irradiation time was adjusted to 0.5 min, and other conditions remained unchanged.

[0093] In this comparative example, after microwave treatment, a lead smelting water-quenched slag-based cementitious material was obtained; its infinite lateral compressive strength was measured to be 45.2 MPa, corresponding specifically to Figure 2 Compressive strength at 0.5 min irradiation time (abscissa).

[0094] Comparative Example 3

[0095] Compared with Example 1, in this comparative example, only the microwave power is adjusted to 0w, the irradiation time is adjusted to 0min, and other conditions remain unchanged; that is, the solidified product after demoulding is directly used as the smelting water-quenched slag-based alkali-activated cementitious material.

[0096] After microwave treatment, the lead smelting water quenching slag-based cementitious material was obtained in this comparative example; its infinite side compressive strength was measured to be 29.3 MPa, corresponding specifically to Figure 2 The compressive strength of 0min irradiation time (abscissa) and the corresponding Figure 3 Compressive strength at 0W microwave power (abscissa).

[0097] Example 6

[0098] Compared with Example 3, in this embodiment, only the microwave power is adjusted to 560W, and other conditions remain unchanged.

[0099] In this embodiment, after microwave treatment, a lead smelting water-quenched slag-based cementitious material is obtained; its infinite side compressive strength is measured to be 48.3 MPa, specifically corresponding to Figure 3 Compressive strength at 560W microwave power (abscissa).

[0100] Comparative Example 4

[0101] Compared with Example 3, in this comparative example, only the microwave power is adjusted to 350W, and other conditions remain unchanged.

[0102] After microwave treatment, the lead smelting water quenching slag-based cementitious material was obtained in this comparative example; its infinite side compressive strength was measured to be 42.3 MPa, corresponding specifically to Figure 3 Compressive strength at 350W microwave power (abscissa).

[0103] Comparative Example 5

[0104] Compared with Example 3, in this comparative example, only the microwave power is adjusted to 210 W, and other conditions remain unchanged.

[0105] In this comparative example, after microwave treatment, a lead smelting water-quenched slag-based cementitious material was obtained; its infinite side compressive strength was measured to be 38.8 MPa, corresponding specifically to Figure 3 Compressive strength at 210W microwave power (abscissa).

[0106] Comparative Example 6

[0107] Compared with Example 3, in this comparative example, only the microwave power is adjusted to 70W, and other conditions remain unchanged.

[0108] In this comparative example, after microwave treatment, a lead smelting water-quenched slag-based cementitious material was obtained; its infinite lateral compressive strength was measured to be 31.1 MPa, corresponding specifically to Figure 3 Compressive strength at 70W microwave power (abscissa).

[0109] Comparative Example 7

[0110] Compared with Comparative Example 4, in this comparative example, only the modified lead smelting water-quenched slag and the alkali activator in step 2 are replaced with PO 42.5 cement of the same mass, and other conditions remain unchanged; that is, in this comparative example, water and cement are directly mixed according to the water-cement ratio, and the ash in this comparative example refers to PO 42.5 cement.

[0111] After the slurry of this comparative example was cured (cured) for 1 day at a temperature of 25°C and a relative humidity of 95%, the infinite side compressive strength of the cured product was measured to be 20.5 MPa; however, the cured product (PO 42.5 block) cracked during the subsequent microwave treatment, and the structure was completely destroyed. Figure 7 shown.

[0112] Comparative Example 8

[0113] Compared with Comparative Example 3, this comparative example only adjusts the curing (curing) for 1 day at a temperature of 25° C. and a relative humidity of 95% to high-temperature curing (covering with a water-retaining film) at 60° C. for 1 day, and other conditions remain unchanged.

[0114] After high-temperature curing, the comparative example obtained a lead smelting water-quenched slag-based cementitious material; the infinite lateral compressive strength thereof was measured to be 48.1 MPa.

[0115] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing a lead smelting water-quenched slag-based cementitious material based on microwave curing, characterized in that: Includes steps: S1, subjecting the lead smelting water-quenched slag to an activation modification treatment to obtain a pre-treated product; wherein the activation modification treatment comprises: ball milling the lead smelting water-quenched slag; The lead smelting water-quenched slag contains iron, and the mass proportion of the iron in the lead smelting water-quenched slag is 25-30%; S2, mixing the pretreated material, an alkali activator and water to obtain a slurry; wherein the preparation components of the alkali activator include water glass and sodium hydroxide; the water glass modulus of the alkali activator is 1-1.5; The mass ratio of the pretreatment material to the alkaline activator is 88-95:5-12; The water: the sum of the pre-treated material and the alkaline activator is 0.15-0.25 mL: 1 g; S3, curing the slurry to obtain a cured product; S4, subjecting the solidified product to microwave treatment to obtain a lead smelting water-quenched slag-based gelling material; wherein the microwave power of the microwave treatment is 560-700 W, and the irradiation time of the microwave treatment is 1-3 min.

2. The preparation method according to claim 1, characterized in that: The activation modification treatment further comprises: before the ball milling, grinding the lead smelting water-quenched slag; The ground lead smelting water-quenched slag is passed through a 20-50 mesh sieve, and the sieve residue is subjected to ball milling.

3. The preparation method according to claim 2, characterized in that: The grinding is carried out in a vibration mill, and the vibration grinding time of the lead smelting water-quenched slag in the vibration mill is 30-120 s.

4. The preparation method according to claim 2, characterized in that: The activation modification treatment further comprises: passing the ball-milled product through a 100-200 mesh sieve, and taking the sieve-down material as the pre-treated material.

5. The preparation method according to claim 1, characterized in that: In the ball milling, the ball milling speed is 250-350 r / min, the ball-to-material mass ratio is 4-12:1, and the ball milling time is 30-60 min.

6. The preparation method according to claim 1, characterized in that: The curing treatment comprises: curing and molding the slurry in a mold to obtain a cured product.

7. The preparation method according to claim 1, characterized in that: The microwave frequency of the microwave treatment is 2450 MHz.

8. A lead smelting water-quenched slag-based cementitious material, characterized in that: The preparation is carried out by the preparation method according to any one of claims 1 to 7.

9. Use of the lead smelting water-quenched slag-based cementitious material as claimed in claim 8 in construction projects.

Citation Information

Cited By

  • Activation modification method of lead smelting water-quenched slag and application of activation modification method

    CN122482734A