A porous ceramic ball material and its preparation method and application
By using porous ceramic ball materials in fuel, including components such as tourmaline and modified activated carbon, the problems of fuel additive pollution and colloid deposition are solved, and efficient combustion and environmentally friendly fuel catalytic effects are achieved, and the service life of the engine is extended .
Patent Information
- Application Number
- CN202310382990.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-04-12
AI Technical Summary
Existing fuel additives produce polluted gases during combustion, resulting in environmental pollution and reduce engine performance. They cannot effectively inhibit colloid deposition in fuel, affecting the service life of the engine.
Porous ceramic ball materials, including tourmaline, calcium carbonate, modified cerium-zirconium composite oxide, lanthanum modified iron oxide, iron spinel, metal dysprosium and zinc sulfate modified activated carbon, reduce fuel molecules by radiating far infrared rays. The agglomeration state improves the atomization quality, and promotes the full combustion of fuel through oxygen storage and oxygen release functions, adsorbs colloids, and reduces the formation of carbon deposits.
Improves fuel combustion efficiency, reduces harmful gas emissions, extends the engine service life, reduces maintenance costs, and is environmentally friendly and does not produce additional polluted gases.
Smart Images

Figure BDA0004172890190000121 
Figure BDA0004172890190000131 
Figure BDA0004172890190000132
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fuel catalysts, and in particular to a porous ceramic ball material and a preparation method and application thereof. Background Art
[0002] During the storage and transportation of fuel, oxidation will occur to generate incombustible colloids. These colloids are easily deposited in the oil pipes, filters, carburetor nozzles and fuel injectors, affecting the normal use of the engine. When these colloids enter the engine together with the fuel, they will gradually deposit on the top of the piston, harden after warm burning, increase combustion carbon deposits, block the oil circuit, and cause undesirable results such as low fuel supply, poor atomization effect, and low concentration of combustible mixed gas, thereby causing a decrease in engine power. In addition, carbon deposits will also reduce the area of the combustion chamber, reduce power, and cause deflagration and knock, affecting the service life of the engine. Therefore, reducing the generation of colloid carbon and ensuring the normal operation of the engine are of great significance for reducing automobile maintenance costs and increasing the service life of the engine.
[0003] Moreover, since motor vehicle fuel contains large molecular clusters, incomplete combustion is prone to occur, resulting in a large amount of combustible harmful gases in its exhaust gas, such as carbon monoxide CO, nitrogen oxides NOx and hydrocarbons, which not only leads to a waste of fuel energy, but also causes more serious environmental pollution problems. In order to achieve the purpose of saving fuel, reducing carbon deposits and purifying exhaust gas, many fuel oil additives have been developed. The current fuel additives mainly add a variety of organic additives to the fuel to quickly decompose the fuel inside the engine and reduce carbon deposits, but this catalyst reduces engine performance; secondly, these additives will produce carbon monoxide, sulfur dioxide and other polluting gases during the combustion process, causing environmental pollution and poor environmental protection. Summary of the invention
[0004] In view of this, the present invention provides a porous ceramic ball material and its preparation method and application. The present invention uses tourmaline as the main raw material, adds calcium carbonate, cerium zirconium composite oxide, modified iron oxide, iron spinel, rare earth metal dysprosium and modified activated carbon, and prepares a porous ceramic material. Using it as a fuel catalyst can promote more complete combustion of fuel, enhance fuel combustion efficiency, and inhibit carbon deposit formation, extend the service life of the engine, and reduce vehicle maintenance costs.
[0005] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0006] A porous ceramic ball material comprises the following components in percentage by mass: 60% to 70% tourmaline, 10% to 20% calcium carbonate, 1% to 3% modified cerium-zirconium composite oxide, 4% to 6% lanthanum-modified iron oxide, 1% to 4% iron spinel, 1% to 2% metal dysprosium powder and 5% to 13% zinc sulfate-modified activated carbon;
[0007] The modified cerium-zirconium composite oxide is a cerium-zirconium composite oxide modified by metal lanthanum, metal praseodymium, metal yttrium, metal calcium and iron hydroxide.
[0008] Compared with the prior art, the porous ceramic ball material provided by the present invention, tourmaline, lanthanum-modified iron oxide and iron spinel can reduce the agglomeration state of fuel molecules by radiating far-infrared rays, and the three can work together to effectively reduce the surface tension of fuel molecules, reduce the particle size of oil droplet atomization droplets, improve the atomization quality, and promote the full combustion of fuel; cerium-zirconium composite oxide has excellent oxygen storage and oxygen release functions, and synergistically with tourmaline, it can significantly increase the oxygen content of fuel, so that the small molecules of fuel cracked by far-infrared rays can be burned more fully; zinc sulfate-modified activated carbon has a large number of microporous structures and stable chemical properties, and can fully absorb colloids and impurities in fuel, improve fuel quality, and zinc sulfate-modified activated carbon can improve the aging resistance of porous ceramic ball materials, thereby increasing the service life of porous ceramic ball materials; rare earth metal dysprosium can accelerate the reaction rate of carbide gas, lanthanum-modified iron oxide and iron spinel to crack fuel molecules, so that the fuel molecules are fully cracked, thereby promoting the full combustion of fuel molecules. Through the synergistic effect of various components, the present invention can efficiently adsorb and purify the fuel that has passed through the porous ceramic ball material, increase the oxygen content of the fuel, and fully crack the fuel molecules, thereby improving the combustion efficiency of the fuel and reducing the emission of harmful gases. At the same time, it can also effectively inhibit the generation of carbon deposits and increase the service life of the engine, and has high practical application value.
[0009] Exemplarily, the particle size of the tourmaline is 2 mm to 5 mm.
[0010] Exemplarily, the particle size of the iron spinel is 7 mm to 15 mm.
[0011] Exemplarily, the particle size of the modified cerium-zirconium composite oxide is 700 μm to 900 μm.
[0012] Exemplarily, the particle size of the lanthanum-modified iron oxide is 100 μm to 120 μm.
[0013] Exemplarily, the particle size of the zinc sulfate modified activated carbon is 0.25 mm to 0.35 mm.
[0014] Preferably, the preparation method of the cerium-zirconium composite oxide comprises the following steps:
[0015] Cerium hydroxide and zirconium hydroxide are mixed evenly, and metal lanthanum, metal praseodymium, metal yttrium, metal calcium and iron hydroxide are added in sequence, mixed evenly, and calcined at 500° C. to 550° C. for 2.0 h to 2.5 h to obtain the modified cerium-zirconium composite oxide.
[0016] Preferably, the mass ratio of the cerium hydroxide to the zirconium hydroxide is 1.25-1.50:1.
[0017] Preferably, the amount of the metal lanthanum added is 4.8% to 5.0% of the mass of cerium hydroxide, the amount of the metal praseodymium added is 4.8% to 5.0% of the mass of cerium hydroxide, the amount of the metal yttrium added is 9.6% to 10.0% of the mass of cerium hydroxide, the amount of the metal calcium added is 0.045% to 0.05% of the mass of cerium hydroxide, and the amount of the iron hydroxide added is 0.045% to 0.05% of the mass of cerium hydroxide.
[0018] Further preferably, the particle size of the cerium hydroxide is 700 μm to 750 μm, the particle size of the zirconium hydroxide is 800 μm to 850 μm, the particle sizes of the metal lanthanum, metal praseodymium, metal yttrium and metal calcium are all 200 μm to 235 μm, and the particle size of the iron hydroxide is 700 μm to 725 μm.
[0019] The preferred cerium-zirconium composite oxide has excellent oxygen release and storage functions, which can provide sufficient oxygen for fuel combustion, promote more thorough combustion of fuel molecules, improve fuel economy, and reduce emissions of pollutants such as carbon monoxide and hydrocarbons in automobile exhaust; and the prepared cerium-zirconium composite oxide can also emit far-infrared rays, destroy hydrogen bonds between hydrocarbon molecular fuels, reduce the degree of association between hydrocarbon fuel molecules, generate small molecule hydrocarbon fuels, and further promote thorough combustion of fuel molecules; at the same time, the preferred cerium-zirconium composite oxide also has excellent anti-aging properties, which can increase the service life of the porous ceramic ball material.
[0020] Preferably, the preparation method of the lanthanum-modified iron oxide comprises the following steps:
[0021] Add ferrous oxide and metallic lanthanum to ferrosoferric oxide in sequence and mix them evenly, press them into shape in a magnetic field, and then sinter them at 1000° C. to 1200° C. for 3 h to 6 h in an inert atmosphere to obtain the lanthanum-modified iron oxide.
[0022] Preferably, the amount of ferric oxide added is 20% to 30% of the mass of ferrosoferric oxide.
[0023] Preferably, the added amount of the metallic lanthanum is 5% to 10% of the total mass of ferrosoferric oxide and ferric oxide.
[0024] Preferably, the intensity of the magnetic field is 2T to 3T.
[0025] Preferably, the particle sizes of the ferrosoferric oxide and ferrous oxide are both 100 μm to 120 μm, and the particle size of the metallic lanthanum is 300 nm to 600 nm.
[0026] The preferred lanthanum-modified iron oxide has stronger magnetism and the ability to radiate far-infrared rays. It can reduce the agglomeration state of fuel molecules, reduce the surface tension of fuel molecules, reduce the particle size of oil droplet atomization droplets, improve atomization quality, and enhance vehicle power by radiating far-infrared rays.
[0027] Preferably, the method for preparing the iron spinel comprises the following steps:
[0028] Magnesium oxide, ferric oxide, aluminum oxide and metal yttrium are uniformly mixed, water is added to the mixture, pressed into shape, dried, melted at 2860° C. to 3500° C., cooled, and crushed to obtain the iron spinel.
[0029] Further preferably, the mass ratio of magnesium oxide to aluminum oxide is 1:2.3-2.9.
[0030] Further preferably, the mass ratio of ferric oxide to aluminum oxide is 1:2.1-2.6.
[0031] Further preferably, the added amount of the metal yttrium is 5% to 7% of the total mass of magnesium oxide, iron oxide and aluminum oxide.
[0032] Adding a specific amount of metal yttrium powder can promote the melting effect and enhance the stability of the performance of the prepared porous ceramic ball material.
[0033] More preferably, the melting time is 12 h to 15 h.
[0034] More preferably, the particle sizes of the magnesium oxide, iron oxide and aluminum oxide are all 80 μm to 100 μm, and the particle size of the metal yttrium is 50 μm to 70 μm.
[0035] Exemplarily, the molten material is cooled at room temperature for 1 to 2 days and then pulverized to a particle size of 7 mm to 15 mm.
[0036] The iron spinel prepared by the above method works synergistically with tourmaline and modified cerium-zirconium composite oxide to further reduce the agglomeration state of fuel molecules, enhance the radiation effect of far infrared rays, improve the atomization effect, and promote the full combustion of fuel.
[0037] Preferably, the preparation method of the zinc sulfate modified activated carbon comprises the following steps:
[0038] Step a, crushing the dried coconut shell carbon powder, and roasting at 650° C. to 750° C. for 4 h to 5 h in a hydrogen atmosphere to obtain pretreated coconut shell carbon powder;
[0039] Step b, adding the pretreated coconut shell carbon powder into a zinc sulfate solution, immersing at 50° C. to 80° C. for 1.5 h to 3 h, filtering, drying, and crushing to obtain the zinc sulfate modified activated carbon.
[0040] Further preferably, the concentration of the zinc sulfate solution is 3 mol / L to 5 mol / L, and the mass ratio of the zinc sulfate solution to the pretreated coconut shell carbon powder is 1:0.25 to 0.35.
[0041] Exemplarily, in step a, the coconut shell carbon powder is crushed to 0.15 mm to 0.25 mm.
[0042] Exemplarily, in step a, the flow rate of hydrogen is 500 mL / min to 600 mL / min.
[0043] Exemplarily, in step b, the powder is crushed to a particle size of 0.25 mm to 0.35 mm.
[0044] The present invention allows hydrogen molecules to penetrate the internal pores of coconut shell carbon powder through the atmosphere of hydrogen flow, fully contact with carbon molecules and form chemical bonds with carbon molecules, thereby inhibiting the oxidation of the carbon powder itself, so that the prepared coconut shell carbon powder has a large specific surface area and a developed pore structure, and subsequently the coconut shell carbon powder is modified by zinc sulfate impregnation, which significantly improves the adsorption capacity of the modified activated carbon, so that the modified activated carbon fully adsorbs impurities and colloids in the fuel, greatly reduces carbon deposits in the engine, and improves the service life of the engine; at the same time, by modifying the activated carbon with zinc sulfate, the chemical properties of the activated carbon can be made more stable, and the reaction of the activated carbon with the fuel molecules can be avoided.
[0045] The present invention also provides a method for preparing a porous ceramic ball material, comprising the following steps:
[0046] Weigh each component according to the designed ratio, mix the weighed tourmaline, calcium carbonate, cerium-zirconium composite oxide, lanthanum-modified iron oxide, iron spinel, metal dysprosium powder and zinc sulfate-modified activated carbon uniformly, granulate, dry, and obtain a pellet;
[0047] The ball blank is placed in a muffle furnace, first heated to 500°C-600°C at a rate of 3°C / min-5°C / min, then heated to 1200°C-1500°C at a rate of 9°C / min-11°C / min, kept warm for 2h-4h, and cooled to obtain the porous ceramic ball material.
[0048] Exemplarily, the particle size of the ball blank is 20 mm to 30 mm.
[0049] Exemplarily, the drying method is specifically: first air-drying for 20 hours to 24 hours, and then drying at 110° C. to 120° C. for 10 hours to 12 hours.
[0050] The preparation method of the porous ceramic ball material provided by the present invention has the advantages of large specific surface area, large adsorption capacity and porosity, and has an excellent effect of catalyzing the combustion of fuel molecules. It can also fully remove impurities and colloids in the fuel molecules, improve the quality of fuel molecules, reduce engine carbon deposits, and increase the service life of the engine. The preparation process of the porous ceramic ball material is simple, easy to operate, low cost, and suitable for industrial-scale production and application.
[0051] The present invention also provides the use of any of the porous ceramic ball materials described above as a fuel catalyst, wherein the porous ceramic ball material is placed in an automobile fuel catalyst, and the automobile fuel catalyst is installed at the front end of the fuel inlet of the automobile fuel filter.
[0052] Exemplarily, 40 to 45 of the porous ceramic ball materials are placed in each fuel catalyst.
[0053] When the porous ceramic ball material prepared by the present invention is used, it only needs to be directly placed in the automobile fuel catalyst, and then the fuel catalyst is installed at the front end of the oil inlet of the automobile filter. The porous ceramic ball material adsorbs and purifies the fuel flowing through, polymerizes the colloid in the fuel, increases the oxygen content of the fuel, releases far-infrared rays to crack the fuel molecules and reduce the surface tension of the fuel. The catalyzed fuel enters the oil circuit and is sprayed into the cylinder, so that the fuel and air are fully mixed, the full combustion of the fuel is promoted, and the emission of harmful gases is reduced; when the polymerized molecules of the colloid exceed the adsorption capacity of the activated carbon, the polymerized colloid molecules will be washed by the fuel, fall off from the surface of the modified activated carbon, flow into the automobile filter with the oil circuit, and are filtered and intercepted by the automobile filter to prevent them from entering the internal combustion engine to burn and form carbon deposits, affecting the efficiency of the engine. The fuel catalyst is easy to install, does not change the structure and performance of the engine combustion chamber, and does not produce additional gases such as carbon monoxide and sulfur dioxide that pollute the environment. It is a green, environmentally friendly and efficient fuel catalyst material with broad application prospects. DETAILED DESCRIPTION
[0054] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0055] In order to better illustrate the present invention, further examples are given below.
[0056] Example 1
[0057] An embodiment of the present invention provides a porous ceramic ball material, comprising the following components in percentage by mass: 70% tourmaline, 10% calcium carbonate, 1% modified cerium-zirconium composite oxide, 4% lanthanum-modified iron oxide, 1% iron spinel, 1% metal dysprosium powder and 13% zinc sulfate-modified activated carbon.
[0058] The preparation method of the porous ceramic ball material specifically comprises the following steps:
[0059] (1) Preparation of modified cerium-zirconium composite oxide:
[0060] Cerium hydroxide powder and zirconium hydroxide powder are mixed evenly in a mass ratio of 1.25:1, and metal element powders of lanthanum, praseodymium and yttrium are added to the above mixture at 4.8%, 5% and 10% of the mass of cerium hydroxide, respectively, and mixed evenly. Then, iron hydroxide and metal element calcium powder are added to the mixture at 0.05% and 0.05% of the mass of cerium hydroxide, respectively, and mixed evenly. The obtained solid mixture is put into a quartz crucible, roasted at 500°C for 2.5 hours, cooled, and crushed to a particle size of 700μm to 900μm to obtain a modified cerium-zirconium composite oxide.
[0061] (2) Preparation of lanthanum-modified iron oxide:
[0062] Add ferric oxide powder to ferroferric oxide powder in an amount of 30% of the mass of ferroferric oxide, then add metal element lanthanum powder to the mixture in an amount of 5% of the total mass of ferroferric oxide and ferric oxide, press into shape in a 2T magnetic field, then place in a vacuum sintering furnace, sinter at 1200°C for 3h, cool, and crush to a particle size of 100μm to 120μm to obtain lanthanum modified iron oxide.
[0063] (3) Preparation of iron spinel:
[0064] The magnesium oxide powder and the aluminum oxide powder are mixed evenly in a mass ratio of 1:2.9, and ferric oxide is added to the above mixture and mixed evenly, the mass ratio of ferric oxide to aluminum oxide is 1:2.1, to obtain a mixed material; then, 7% of the total mass of the mixed material is added with metal yttrium powder, and the mixture is put into a dry powder mixer and stirred for 1 hour, and then put into a ball press machine and press it with water, and then put it into an electric blast drying oven and dry it at 120°C for 1 hour, and the dried molded material is put into a smelting furnace, melted at 3500°C for 12 hours, and then cooled at room temperature for 2 days, and crushed to a particle size of 7mm to 15mm to obtain iron spinel.
[0065] (4) Preparation of zinc sulfate modified activated carbon:
[0066] The coconut shell carbon powder was washed with distilled water, filtered, dried at 110°C for 2h, crushed to particles with a particle size of 0.15-0.25mm, and then roasted at 750°C for 4h in an atmosphere with a hydrogen flow rate of 600mL / min to obtain pretreated coconut shell carbon powder; the pretreated coconut shell carbon powder was then placed in a 3mol / L zinc sulfate solution with a mass ratio of pretreated coconut shell carbon powder to zinc sulfate of 0.25:1, immersed at 50°C for 3h, filtered, dried at 110°C for 24h, crushed to particles with a particle size of 0.25-0.35mm, and zinc sulfate-modified activated carbon was obtained.
[0067] (5) Preparation of porous ceramic ball materials:
[0068] Weigh each component according to the designed ratio, mix the weighed tourmaline, calcium carbonate, cerium-zirconium composite oxide, lanthanum-modified iron oxide, iron spinel, metal dysprosium powder and zinc sulfate-modified activated carbon evenly, put them into a spherical particle forming machine, use a rolling forming method to granulate, obtain spherical particles with a particle size of 20-30 mm, naturally air-dry for 20 hours, and then place them in a 120° C. electric heating blast drying oven for 10 hours to obtain a ball blank;
[0069] The ball blank is placed in a muffle furnace, first heated to 500° C. at a rate of 3° C. / min, then heated to 1200° C. at a rate of 9° C. / min, kept warm for 4 hours, and cooled along with the furnace to obtain the porous ceramic ball material.
[0070] Example 2
[0071] The embodiment of the present invention provides a porous ceramic ball material, comprising the following components in percentage by mass: 60% tourmaline, 20% calcium carbonate, 3% modified cerium-zirconium composite oxide, 6% lanthanum-modified iron oxide, 4% iron spinel, 2% metal dysprosium powder and 5% zinc sulfate-modified activated carbon.
[0072] The preparation method of the porous ceramic ball material specifically comprises the following steps:
[0073] (1) Preparation of modified cerium-zirconium composite oxide:
[0074] Cerium hydroxide powder and zirconium hydroxide powder are mixed evenly in a mass ratio of 1.5:1, and metal element powders of lanthanum, praseodymium and yttrium are added to the above mixture at a mass ratio of 5%, 4.9% and 9.6% of the mass of cerium hydroxide, respectively, and mixed evenly. Then, iron hydroxide and metal element calcium powder are added to the mixture at a mass ratio of 0.045% and 0.048% of the mass of cerium hydroxide, respectively, and mixed evenly. The obtained solid mixture is put into a quartz crucible, calcined at 550°C for 2h, cooled, and crushed to a particle size of 700μm to 900μm to obtain a modified cerium-zirconium composite oxide.
[0075] (2) Preparation of lanthanum-modified iron oxide:
[0076] Add ferric oxide powder to ferroferric oxide powder in an amount of 20% of the mass of ferroferric oxide, then add metal element lanthanum powder to the mixture in an amount of 10% of the total mass of ferroferric oxide and ferric oxide, press into shape in a 3T magnetic field, then place in a vacuum sintering furnace, sinter at 1000°C for 6h, cool, and crush to a particle size of 100μm to 120μm to obtain lanthanum modified iron oxide.
[0077] (3) Preparation of iron spinel:
[0078] The magnesium oxide powder and the aluminum oxide powder are mixed evenly in a mass ratio of 1:2.3, and ferric oxide is added to the above mixture and mixed evenly, the mass ratio of ferric oxide to aluminum oxide is 1:2.6, to obtain a mixed material; then 5% of the total mass of the mixed material is added with metal yttrium powder, and the mixture is put into a dry powder mixer and stirred for 0.5h, and then put into a ball press machine and press it with water, and then put it into an electric blast drying oven and dry it at 100°C for 1.5h, put the dried molded material into a smelting furnace, melt it at 2860°C for 15h, and then cool it at room temperature for 1 day, and crush it to a particle size of 7mm to 15mm to obtain iron spinel.
[0079] (4) Preparation of zinc sulfate modified activated carbon:
[0080] The coconut shell carbon powder was washed with distilled water, filtered, dried at 120°C for 1h, crushed to particles with a particle size of 0.15-0.25mm, and then roasted at 650°C for 5h in an atmosphere with a hydrogen flow rate of 500mL / min to obtain pretreated coconut shell carbon powder; the pretreated coconut shell carbon powder was then placed in a 5mol / L zinc sulfate solution with a mass ratio of pretreated coconut shell carbon powder to zinc sulfate of 0.35:1, immersed at 80°C for 1.5h, filtered, dried at 120°C for 20h, crushed to particles with a particle size of 0.25-0.35mm, and zinc sulfate-modified activated carbon was obtained.
[0081] (5) Preparation of porous ceramic ball materials:
[0082] Weigh each component according to the designed ratio, mix the weighed tourmaline, calcium carbonate, cerium-zirconium composite oxide, lanthanum-modified iron oxide, iron spinel, metal dysprosium powder and zinc sulfate-modified activated carbon evenly, put them into a spherical particle forming machine, use a rolling forming method to granulate, obtain spherical particles with a particle size of 20-30 mm, naturally air-dry for 24 hours, and then place them in an electric heating blast drying oven at 110° C. to dry for 12 hours to obtain a ball blank;
[0083] The ball blank is placed in a muffle furnace, first heated to 600° C. at a rate of 5° C. / min, then heated to 1500° C. at a rate of 11° C. / min, kept warm for 2 hours, and cooled along with the furnace to obtain the porous ceramic ball material.
[0084] Example 3
[0085] An embodiment of the present invention provides a porous ceramic ball material, comprising the following components in percentage by mass: 65% tourmaline, 15% calcium carbonate, 2% modified cerium-zirconium composite oxide, 5% lanthanum-modified iron oxide, 3% iron spinel, 2% metal dysprosium powder and 8% zinc sulfate-modified activated carbon.
[0086] The preparation method of the porous ceramic ball material specifically comprises the following steps:
[0087] (1) Preparation of modified cerium-zirconium composite oxide:
[0088] Cerium hydroxide powder and zirconium hydroxide powder are mixed evenly in a mass ratio of 1.4:1, and metal element powders of lanthanum, praseodymium and yttrium are added to the above mixture at 4.9%, 4.8% and 9.8% of the mass of cerium hydroxide, respectively, and mixed evenly. Then, iron hydroxide and metal element calcium powder are added to the mixture at 0.048% and 0.045% of the mass of cerium hydroxide, respectively, and mixed evenly. The obtained solid mixture is put into a quartz crucible, roasted at 530°C for 2.5 hours, cooled, and crushed to a particle size of 700μm to 900μm to obtain a modified cerium-zirconium composite oxide.
[0089] (2) Preparation of lanthanum-modified iron oxide:
[0090] Add ferric oxide powder to ferroferric oxide powder in an amount of 25% of the mass of ferroferric oxide, then add metal element lanthanum powder to the mixture in an amount of 8% of the total mass of ferroferric oxide and ferric oxide, press into shape in a 2.5T magnetic field, then place in a vacuum sintering furnace, sinter at 1100°C for 4h, cool, and crush to a particle size of 100μm to 120μm to obtain lanthanum modified iron oxide.
[0091] (3) Preparation of iron spinel:
[0092] The magnesium oxide powder and the aluminum oxide powder are mixed evenly in a mass ratio of 1:2.5, and ferric oxide is added to the above mixture and mixed evenly, the mass ratio of ferric oxide to aluminum oxide is 1:2.3, to obtain a mixed material; then, 6% of the total mass of the mixed material is added with metal yttrium powder, and the mixture is put into a dry powder mixer and stirred for 1 hour, and then put into a ball press machine and press it with water to form it, and then put it into an electric blast drying oven and dry it at 120°C for 1 hour, put the dried molded material into a smelting furnace, melt it at 3000°C for 14 hours, and then cool it at room temperature for 1 day, and crush it to a particle size of 7mm to 15mm to obtain iron spinel.
[0093] (4) Preparation of zinc sulfate modified activated carbon:
[0094] The coconut shell carbon powder was washed with distilled water, filtered, dried at 120°C for 1h, crushed to particles with a particle size of 0.15-0.25mm, and then roasted at 700°C for 4.5h in an atmosphere with a hydrogen flow rate of 550mL / min to obtain pretreated coconut shell carbon powder; then the pretreated coconut shell carbon powder was placed in a 4mol / L zinc sulfate solution with a mass ratio of pretreated coconut shell carbon powder to zinc sulfate of 0.3:1, immersed at 65°C for 2h, filtered, dried at 120°C for 20h, crushed to particles with a particle size of 0.25-0.35mm, and zinc sulfate-modified activated carbon was obtained.
[0095] (5) Preparation of porous ceramic ball materials:
[0096] Weigh each component according to the designed ratio, mix the weighed tourmaline, calcium carbonate, cerium-zirconium composite oxide, lanthanum-modified iron oxide, iron spinel, metal dysprosium powder and zinc sulfate-modified activated carbon evenly, put them into a spherical particle forming machine, use a rolling forming method to granulate, obtain spherical particles with a particle size of 20-30 mm, naturally air-dry for 24 hours, and then place them in a 120° C. electric heating blast drying oven for 10 hours to obtain a ball blank;
[0097] The ball blank is placed in a muffle furnace, first heated to 550°C at a rate of 4°C / min, then heated to 1350°C at a rate of 10°C / min, kept at this temperature for 3 hours, and cooled along with the furnace to obtain the porous ceramic ball material.
[0098] Comparative Example 1-Comparative Example 3
[0099] This comparative example provides a porous ceramic ball material, the raw material composition and preparation method of which are the same as those of Examples 1-3, except that the zinc sulfate-modified activated carbon in Examples 1-3 is replaced by a corresponding amount of copper nitrate-modified activated carbon, and the preparation method of the copper nitrate-modified activated carbon is as follows:
[0100] The coconut shell carbon powder was washed with distilled water, filtered, dried at 120°C for 1h, crushed to particles with a particle size of 0.15-0.25mm, and then calcined at 700°C for 4.5h in an atmosphere with a hydrogen flow rate of 550mL / min to obtain pretreated coconut shell carbon powder; then the pretreated coconut shell carbon powder was placed in a 4mol / L copper nitrate solution with a mass ratio of the pretreated coconut shell carbon powder to zinc sulfate of 0.3:1, immersed at 65°C for 2h, filtered, dried at 120°C for 20h, crushed to particles with a particle size of 0.25-0.35mm, and copper nitrate modified activated carbon was obtained.
[0101] The porous ceramic ball material was prepared in the same manner as in Example 3.
[0102] Comparative Example 4-Comparative Example 6
[0103] This comparative example provides a porous ceramic ball material, the raw material composition and preparation method of which are the same as those of Examples 1-3, except that the lanthanum-modified iron oxides of Examples 1-3 are replaced by corresponding equivalent amounts of copper-modified iron oxides, and the preparation method of the copper-modified iron oxides is as follows:
[0104] Add ferric oxide powder to ferroferric oxide powder in an amount of 25% of the mass of ferroferric oxide, then add metallic copper powder to the mixture in an amount of 8% of the total mass of ferroferric oxide and ferric oxide, press into shape in a 2.5T magnetic field, then place in a vacuum sintering furnace, sinter at 1100°C for 4h, cool, and crush to a particle size of 100μm to 120μm to obtain copper-modified iron oxide.
[0105] The porous ceramic ball material was prepared in the same manner as in Example 3.
[0106] Performance Testing
[0107] A car with 0 kilometers of driving was used, gasoline was used as raw material, and low idling speed was used for testing. The porous ceramic ball material prepared in the embodiment and the comparative example was placed in an automobile fuel catalyst, and the automobile fuel catalyst was installed at the front end of the fuel inlet of the automobile fuel filter. 40 porous ceramic balls were placed in each fuel catalyst, and a control group was set up without adding porous ceramic balls.
[0108] After implementation, the vehicle will be tested on the spot by idling for 30 minutes, then tested once a month for 4 consecutive months, and a follow-up test will be conducted after 1 year.
[0109] The test instrument is Foshan Analytical Instrument Co., Ltd. FGA4100 automobile exhaust analyzer, which complies with GB18285-2005 and GB3847-2005 standards. The test results are shown in Table 1.
[0110] Three Accord 230TURBO1.5T cars with a mileage of 0 kilometers were used, two of which were respectively placed with 40 porous ceramic balls prepared in Example 1 and Comparative Example 1, and the other one was not placed with porous ceramic balls.
[0111] Table 1
[0112]
[0113]
[0114] Test 2
[0115] Three Trumpchi GS41.5T cars with a mileage of 0 kilometers were used, two of which were respectively placed with 40 porous ceramic balls prepared in Example 2 and Comparative Example 2, and the other one was not placed with porous ceramic balls.
[0116] Table 2
[0117]
[0118]
[0119] Test 3
[0120] Three Mercedes-Benz G500s with a mileage of 0 kilometers and a displacement of 4.0 V8 engine were used, two of which were respectively equipped with 40 porous ceramic balls prepared in Example 3 and Comparative Example 3, and the other one was not equipped with porous ceramic balls.
[0121] Table 3
[0122]
[0123]
[0124] Test 4
[0125] Three Ford Focus cars with a mileage of 0 kilometers and a displacement of 1.8 were used, two of which were respectively equipped with 40 porous ceramic balls prepared in Example 1 and Comparative Example 4, and the other one was not equipped with any porous ceramic balls.
[0126] Table 4
[0127]
[0128]
[0129] Test 5
[0130] Three GAC Toyota Highlander 2.7 vehicles with a mileage of 0 kilometers were used, two of which were respectively equipped with 40 porous ceramic balls prepared in Example 2 and Comparative Example 5, and the other one was not equipped with porous ceramic balls.
[0131] Table 5
[0132]
[0133]
[0134] Test 6
[0135] Three American imported Jeep Liberty vehicles with a mileage of 0 kilometers and a displacement of 3.7V6 engine were used. Two of them were respectively equipped with 40 porous ceramic balls prepared in Example 3 and Comparative Example 6, and the other one was not equipped with porous ceramic balls.
[0136] Table 6
[0137]
[0138] The particle sizes of the materials used in the above-mentioned embodiments and comparative examples are as follows:
[0139] The particle size of the cerium hydroxide is 700μm to 750μm, the particle size of the zirconium hydroxide is 800μm to 850μm, the particle sizes of the metal lanthanum, metal praseodymium, metal yttrium and metal calcium are all 200μm to 235μm, and the particle size of the iron hydroxide is 700μm to 725μm; the particle sizes of the ferroferric oxide and ferric oxide are both 100μm to 120μm, and the particle size of the metal lanthanum is 300nm to 600nm; the particle sizes of the magnesium oxide, iron oxide and aluminum oxide are all 80μm to 100μm, and the particle size of the metal yttrium is 50μm to 70μm.
[0140] The materials prepared within the above-mentioned particle size range can achieve basically equivalent technical effects.
[0141] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A porous ceramic ball material, It is characterized in that The invention comprises the following components in percentage by mass: 60% to 70% of tourmaline, 10% to 20% of calcium carbonate, 1% to 3% of modified cerium-zirconium composite oxide, 4% to 6% of lanthanum-modified iron oxide, 1% to 4% of iron spinel, 1% to 2% of metal dysprosium powder and 5% to 13% of zinc sulfate-modified activated carbon; The modified cerium-zirconium composite oxide is a cerium-zirconium composite oxide modified by metal lanthanum, metal praseodymium, metal yttrium, metal calcium and iron hydroxide; The preparation method of the lanthanum modified iron oxide comprises the following steps: Add ferrous oxide and metallic lanthanum to ferrosoferric oxide in sequence and mix them evenly, press them into shape in a magnetic field, and then sinter them at 1000° C. to 1200° C. for 3 h to 6 h in an inert atmosphere to obtain the lanthanum-modified iron oxide.
2. The porous ceramic ball material according to claim 1, It is characterized in that The preparation method of the cerium-zirconium composite oxide comprises the following steps: Cerium hydroxide and zirconium hydroxide are mixed evenly, and metal lanthanum, metal praseodymium, metal yttrium, metal calcium and iron hydroxide are added in sequence, mixed evenly, and calcined at 500° C. to 550° C. for 2.0 h to 2.5 h to obtain the modified cerium-zirconium composite oxide.
3. The porous ceramic ball material as claimed in claim 2, It is characterized in that The mass ratio of cerium hydroxide to zirconium hydroxide is 1.25-1.50:1; and / or The amount of the metal lanthanum added is 4.8% to 5.0% of the mass of the cerium hydroxide, the amount of the metal praseodymium added is 4.8% to 5.0% of the mass of the cerium hydroxide, the amount of the metal yttrium added is 9.6% to 10.0% of the mass of the cerium hydroxide, the amount of the metal calcium added is 0.045% to 0.05% of the mass of the cerium hydroxide, and the amount of the iron hydroxide added is 0.045% to 0.05% of the mass of the cerium hydroxide; and / or The particle size of the cerium hydroxide is 700 μm to 750 μm, the particle size of the zirconium hydroxide is 800 μm to 850 μm, the particle sizes of the metal lanthanum, metal praseodymium, metal yttrium and metal calcium are all 200 μm to 235 μm, and the particle size of the iron hydroxide is 700 μm to 725 μm.
4. The porous ceramic ball material according to claim 1, It is characterized in that The amount of ferric oxide added is 20% to 30% of the mass of ferrosoferric oxide; and / or The amount of the metal lanthanum added is 5% to 10% of the total mass of ferrosoferric oxide and ferric oxide; and / or The intensity of the magnetic field is 2T to 3T; and / or The particle sizes of the ferrosoferric oxide and the ferrous oxide are both 100 μm to 120 μm, and the particle size of the metal lanthanum is 300 nm to 600 nm.
5. The porous ceramic ball material according to claim 1, It is characterized in that The preparation method of the iron spinel comprises the following steps: Magnesium oxide, ferric oxide, aluminum oxide and metal yttrium are uniformly mixed, water is added to the obtained mixture, pressed into shape, dried, melted at 2860° C. to 3500° C., cooled, and crushed to obtain the iron spinel.
6. The porous ceramic ball material according to claim 1, It is characterized in that The preparation method of the zinc sulfate modified activated carbon comprises the following steps: Step a, crushing the dried coconut shell carbon powder, and roasting at 650° C. to 750° C. for 4 h to 5 h in a hydrogen atmosphere to obtain pretreated coconut shell carbon powder; Step b, adding the pretreated coconut shell carbon powder into a zinc sulfate solution, immersing at 50° C. to 80° C. for 1.5 h to 3 h, filtering, drying, and crushing to obtain the zinc sulfate modified activated carbon.
7. The porous ceramic ball material according to claim 6, It is characterized in that The concentration of the zinc sulfate solution is 3 mol / L to 5 mol / L, and the mass ratio of the zinc sulfate solution to the pretreated coconut shell carbon powder is 1:0.25 to 0.
35.
8. A method for preparing the porous ceramic ball material according to any one of claims 1 to 7, It is characterized in that The steps include: Weigh each component according to the designed ratio, mix the weighed tourmaline, calcium carbonate, cerium-zirconium composite oxide, lanthanum-modified iron oxide, iron spinel, metal dysprosium powder and zinc sulfate-modified activated carbon uniformly, granulate, dry, and obtain a pellet; The ball blank is placed in a muffle furnace, first heated to 500°C-600°C at a rate of 3°C / min-5°C / min, then heated to 1200°C-1500°C at a rate of 9°C / min-11°C / min, kept warm for 2h-4h, and cooled to obtain the porous ceramic ball material.
9. Use of the porous ceramic ball material according to any one of claims 1 to 7 as a fuel catalyst, It is characterized in that The porous ceramic ball material is placed in an automobile fuel catalyst, and the automobile fuel catalyst is installed at the front end of the fuel inlet of the automobile fuel filter.