An optimized production process and equipment for resorcinol rubber adhesive
By optimizing the production process of resorcinol rubber adhesives, including ultrasonic cleaning, grinding and microwave reactor treatment, combined with additives such as vulcanizing agents, forming a crosslinked structure, the poor stability of the adhesive in the prior art has been solved. Problem, improving the performance and production efficiency of the adhesive.
Patent Information
- Application Number
- CN202310379291.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-04-11
AI Technical Summary
The existing preparation methods of resorcinol rubber adhesives are complex and have insufficient adhesive strength and poor stability, resulting in a reduced service life.
Adopted an optimized production process, including ultrasonic cleaning, grinding treatment, microwave reactor preparation of hydrogenated renewable materials, mixing and calendering cutting, etc., the cross-linked structure is formed through the combination of vulcanizing agent, accelerator, active agent and anti-aging agent. To improve the strength and durability of the adhesive.
It improves the heat resistance, corrosion resistance, wear resistance and adhesion of resorcinol rubber adhesive, while improving production efficiency and extending service life.
Smart Images

Figure CN116376468B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rubber adhesive preparation, and in particular to an optimized production process and equipment for a resorcinol rubber adhesive. Background Art
[0002] Resorcinol rubber adhesive is a rubber adhesive with resorcinol as the main component, usually used to bond rubber products, metals, plastics and other materials. Resorcinol rubber adhesive has the following characteristics:
[0003] Heat resistance: Rubber adhesives can maintain stable performance under high temperature conditions and are not easy to melt or decompose.
[0004] Corrosion resistance: Rubber adhesives are resistant to corrosion and erosion from a variety of chemicals and are not easily damaged.
[0005] Abrasion resistance: Rubber adhesive resists friction and abrasion and is not easy to fall off or peel off.
[0006] Good adhesion: Rubber adhesives can form a strong bond with rubber products and have good adhesion and adhesion.
[0007] Good flexibility: Rubber adhesive has a certain flexibility and elasticity, and can adapt to various complex shapes and deformations.
[0008] Environmental protection: The raw materials and additives used in rubber adhesives are generally environmentally friendly and safe, and will not cause harm to the human body and the environment.
[0009] Rubber adhesives have a wide range of applications and are commonly used in the fields of automobile manufacturing, tire manufacturing, rubber tube manufacturing, building sealing, etc. Different application fields and requirements will require different types of rubber adhesives, so in actual production, they need to be selected and optimized according to specific circumstances.
[0010] The existing preparation method of resorcinol rubber adhesive is too complicated, and the prepared resorcinol rubber adhesive has insufficient bonding strength and poor stability, thereby reducing the service life of resorcinol. Therefore, in view of the above shortcomings, it is necessary to improve the production process of resorcinol rubber adhesive. Summary of the invention
[0011] In order to solve the above technical problems, the present invention provides an optimized production process and equipment for resorcinol rubber adhesive.
[0012] The technical solution of the present invention is: an optimized production process of resorcinol rubber adhesive, comprising the following steps:
[0013] S1. Raw material preparation:
[0014] Take 20-50 parts of resorcinol, 50-80 parts of chloroprene rubber, 8-10 parts of hydrogenated renewable materials, 3-5 parts of vulcanizing agent, 1-3 parts of accelerator, 2-5 parts of active agent, and 1-3 parts of antioxidant according to the following weight parts;
[0015] S2. Rubber pretreatment:
[0016] The chloroprene rubber is cleaned by ultrasonic wave, and then crushed by grinding device, and then dried to obtain rubber powder;
[0017] S3. Preparation of hydrogenated renewable materials:
[0018] The palm oil and potassium hydroxide are uniformly mixed in a mass ratio of 10:1, and then put into a microwave reactor for heating reaction. The heating temperature is 100-200°C, and the reaction time is 1-3 hours. After the reaction, pure water is added. The mass ratio of pure water to palm oil is 3:10. The mixture is stirred at a stirring speed of 80-120 r / min for 20-30 minutes, and then an extraction treatment is performed to remove pure water to obtain a hydrogenated renewable material;
[0019] S4, raw material mixing:
[0020] Add rubber powder, hydrogenated renewable materials, resorcinol, vulcanizing agent, accelerator, activator, and antioxidant into a mixer according to the weight portions described in step S1 for mixing. The mixing time is 1-2 hours and the mixing speed is 120-180 rpm. After the mixing is completed, a mixture is obtained.
[0021] S5. Mixing:
[0022] The mixture obtained in step S4 is placed in a mixer for mixing at a mixing speed of 60-120 rpm, the temperature is raised to 80-120° C. at a heating rate of 5-8° C. / min, mixing is started, and the mixing time is 30-40 min. After the mixing is completed, a mixed material is obtained;
[0023] S6, calendering and cutting:
[0024] The mixed material is put into a calender for calendering at a calendering temperature of 100-120°C. The mixed material forms a sheet-like mixed material under the pressure of the calender roller. The sheet-like mixed material is air-cooled to -3-5°C. After cooling, the sheet-like mixed material is cut to obtain a resorcinol rubber adhesive.
[0025] Furthermore, the vulcanizing agent is prepared by mixing ammonium sulfate and sodium hydrogen sulfide in a mass ratio of 1:1.
[0026] Description: Under the action of the vulcanizing agent, the double bonds in the rubber will break, forming a cross-linked structure, thereby forming a strong network structure between the rubber molecules. The vulcanization reaction can improve the strength and durability of the rubber adhesive, thereby enhancing its bonding ability and service life.
[0027] Furthermore, the accelerator is prepared by mixing zinc sulfate, phenylpropyl ketone and epoxy resin in a mass ratio of 1:2:1.
[0028] Description: The above accelerator can improve the performance of rubber adhesive after vulcanization, and improve the hardness, elasticity, durability, heat resistance, cold resistance and other properties of rubber adhesive, so that the rubber adhesive has better performance and life.
[0029] Furthermore, the active agent is prepared by mixing hydrogen peroxide and sodium thiosulfate in a mass ratio of 1:3.
[0030] Description: The above-mentioned active agent can effectively help rubber molecules form a strong cross-linking structure, thereby improving the strength, durability and stability of the rubber adhesive.
[0031] Furthermore, the antioxidant is prepared by mixing catechol, dimethyl dithiocarboxylic acid, and isobutyl diphenol in a mass ratio of 1:1:1.
[0032] Note: The above antioxidants can effectively protect rubber molecules from oxidation, thermal decomposition, light and other factors, thereby extending the service life and performance stability of rubber adhesives.
[0033] Furthermore, in the step S2, the frequency of ultrasonic cleaning is 150-200 KHz, the duration of ultrasonic cleaning is 30-40 min, the drying temperature during the drying process is 50-80° C., and the drying time is 10-20 min.
[0034] Note: Ultrasonic cleaning can improve the efficiency of rubber cleaning, and appropriate drying temperature can prevent rubber from softening.
[0035] Furthermore, the rubber powder in step S2 has a particle size of 200-300 μm.
[0036] Note: The particle size of the rubber powder can be effectively mixed with resorcinol to improve the efficiency of raw material mixing.
[0037] Furthermore, the grinding device includes a motor base, a grinding cylinder, a rotating motor, a rotating shaft, a short rod, a cutting cylinder, and a discharge port. The motor base is fixedly connected to the grinding cylinder through the fixed frame, the cutting cylinder is fixedly connected above the grinding cylinder, the rotating motor is fixedly connected inside the motor base, the lower end of the rotating shaft is rotatably connected to the bottom of the grinding cylinder and is transmission-connected to the output shaft of the rotating motor, the upper end of the rotating shaft is rotatably connected to the top of the cutting cylinder through the short rod, a grinding disk is fixedly connected to the outer side of the bottom of the rotating shaft, two fixed plates are fixedly connected above the rotating shaft, a cutting stick is rotatably connected to each of the two sides between the two fixed plates, and the discharge port is fixedly connected to one side of the grinding cylinder.
[0038] Description: The above grinding device can improve the efficiency of rubber grinding and further improve the production efficiency of rubber adhesive.
[0039] Furthermore, the microwave reactor includes a microwave generator, a microwave shell, a microwave chamber, a waveguide, a chamber door, a reaction tube, and a stirring rack. The microwave generator is fixedly installed on the right side of the microwave shell, the microwave chamber is located on the left side of the microwave shell, the microwave chamber and the microwave generator are connected through the waveguide, the chamber door is hinged on the front side of the microwave chamber, the reaction tube is placed inside the microwave chamber, the stirring rack is fixedly connected to the top of the microwave shell and is located above the microwave chamber, two hydraulic rods are fixedly connected to the top of the stirring rack, the lower end of the hydraulic rod is fixedly connected to a hydraulic plate, the top of the hydraulic plate is fixedly connected to a stirring motor, the output shaft of the stirring motor is transmission-connected to the stirring rod, and a sealing ring is provided under the hydraulic plate.
[0040] Description: The above microwave reactor can effectively improve the hydrogenation reaction of palm oil and improve the production efficiency of hydrogenated renewable materials.
[0041] Furthermore, the calender includes a pressing plate, a supporting frame, and a sliding frame. An electronic heating plate is provided at the bottom of the pressing plate. The supporting frame is fixedly connected to the bottom of the pressing plate. There are two sliding frames, which are respectively fixedly connected to both sides of the supporting frame. A sliding block is provided inside the sliding frame. The front and rear outer walls of the sliding block are slidably connected to the sliding frame. An adjusting screw is threadedly connected to the front and rear sides of the sliding block. The upper and lower ends of the adjusting screw are respectively rotatably connected to the upper and lower sides of the sliding frame. A roller is rotatably connected between the two sliding blocks. A calendering motor is provided at one end of the roller. The calendering motor is fixedly connected to the sliding block, and the output shaft of the calendering motor is transmission-connected to the roller.
[0042] Description: The above calender can keep the rubber adhesive softened during the calendering process, thereby improving the efficiency of rubber adhesive calendering.
[0043] The beneficial effects of the present invention are:
[0044] (1) The resorcinol rubber adhesive prepared by the present invention has good heat resistance, corrosion resistance, wear resistance, adhesion and flexibility. At the same time, the production process of the present invention can effectively improve the production efficiency of the resorcinol rubber adhesive.
[0045] (2) The grinding device used in the present invention has high grinding efficiency and small grinding particle size, and can effectively promote the mixing efficiency between raw materials. The microwave reactor used in the present invention has high efficiency in preparing hydrogenated renewable materials, and the calender used in the present invention has high calendering efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 It is a schematic structural diagram of the grinding device of the present invention.
[0047] Figure 2 It is a top view of the cutting barrel in the grinding device of the present invention.
[0048] Figure 3 It is a cross-sectional view of the cutting stick and the cutting cylinder wall in the grinding device of the present invention.
[0049] Figure 4 It is a top view of the grinding disc in the grinding device of the present invention.
[0050] Figure 5 It is a schematic structural diagram of a microwave reaction kettle of the present invention.
[0051] Figure 6 It is a structural schematic diagram of the calender of the present invention.
[0052] Figure 7 It is a process flow chart of the resorcinol rubber adhesive of the present invention.
[0053] Among them, 11-motor base, 12-grinding cylinder, 13-rotating motor, 14-rotating shaft, 15-short rod, 16-cutting cylinder, 17-discharging port, 18-grinding disc, 19-fixed plate, 191-cutting stick, 21-microwave generator, 22-microwave shell, 23-microwave bin, 24-waveguide, 25-bin door, 26-reaction cylinder, 27-stirring frame, 28-hydraulic rod, 29-hydraulic plate, 291-stirring motor, 292-stirring rod, 293-sealing ring, 31-pressing plate, 32-support frame, 33-sliding frame, 34-sliding block, 35-adjusting screw, 36-roller, 37-calendering motor, 311-electronic heating plate. DETAILED DESCRIPTION
[0054] Embodiment 1:
[0055] like Figure 7 As shown, an optimized production process of resorcinol rubber adhesive comprises the following steps:
[0056] S1. Raw material preparation:
[0057] Take 20 parts of resorcinol, 50 parts of chloroprene rubber, 8 parts of hydrogenated renewable materials, 3 parts of vulcanizing agent, 1 part of accelerator, 2 parts of activator, and 1 part of antioxidant according to the following weight parts;
[0058] The vulcanizing agent is prepared by mixing ammonium sulfate and sodium hydrogen sulfide in a mass ratio of 1:1;
[0059] The accelerator is prepared by mixing zinc sulfate, phenylpropyl ketone and epoxy resin in a mass ratio of 1:2:1;
[0060] The active agent is prepared by mixing hydrogen peroxide and sodium thiosulfate in a mass ratio of 1:3;
[0061] The antioxidant is prepared by mixing catechol, dimethyl dithiocarboxylic acid and isobutyl diphenol in a mass ratio of 1:1:1;
[0062] S2. Rubber pretreatment:
[0063] The chloroprene rubber is cleaned by ultrasonic wave, and then crushed by a grinding device, and then dried to obtain rubber powder; the frequency of ultrasonic wave cleaning is 150KHz, the ultrasonic wave cleaning time is 30min, the drying temperature during the drying process is 50℃, the drying time is 10min, and the rubber powder particle size is 200-300μm;
[0064] S3. Preparation of hydrogenated renewable materials:
[0065] Palm oil and potassium hydroxide were mixed evenly at a mass ratio of 10:1, and then placed in a microwave reactor for heating reaction at a heating temperature of 100°C and a reaction time of 1 hour. After the reaction, pure water was added at a mass ratio of pure water to palm oil of 3:10, and stirred at a stirring speed of 80 r / min for 20 minutes, and then extracted to remove pure water to obtain a hydrogenated renewable material;
[0066] S4, raw material mixing:
[0067] Add rubber powder, hydrogenated renewable materials, resorcinol, vulcanizing agent, accelerator, activator, and antioxidant into a mixer according to the weight portions in step S1 for mixing. The mixing time is 1 hour and the mixing speed is 120 rpm. After the mixing is completed, a mixture is obtained.
[0068] S5. Mixing:
[0069] The mixture obtained in step S4 is placed in a mixer for mixing at a mixing speed of 60 rpm, and the temperature is raised to 80° C. at a heating rate of 5° C. / min, and mixing is started for 30 min. After the mixing is completed, a mixed material is obtained;
[0070] S6, calendering and cutting:
[0071] The mixed material is put into a calender for calendering at a calendering temperature of 100°C. The mixed material is formed into a sheet-like mixed material under the pressure of the calender roller 36. The sheet-like mixed material is air-cooled to -3°C. After cooling, the sheet-like mixed material is cut to obtain a resorcinol rubber adhesive.
[0072] Embodiment 2:
[0073] like Figure 7 As shown, an optimized production process of resorcinol rubber adhesive comprises the following steps:
[0074] S1. Raw material preparation:
[0075] Take 35 parts of resorcinol, 60 parts of chloroprene rubber, 9 parts of hydrogenated renewable materials, 4 parts of vulcanizing agent, 2 parts of accelerator, 4 parts of activator, and 2 parts of antioxidant according to the following weight parts;
[0076] The vulcanizing agent is prepared by mixing ammonium sulfate and sodium hydrogen sulfide in a mass ratio of 1:1;
[0077] The accelerator is prepared by mixing zinc sulfate, phenylpropyl ketone and epoxy resin in a mass ratio of 1:2:1;
[0078] The active agent is prepared by mixing hydrogen peroxide and sodium thiosulfate in a mass ratio of 1:3;
[0079] The antioxidant is prepared by mixing catechol, dimethyl dithiocarboxylic acid and isobutyl diphenol in a mass ratio of 1:1:1;
[0080] S2. Rubber pretreatment:
[0081] The chloroprene rubber is cleaned by ultrasonic wave, and then crushed by a grinding device, and then dried to obtain rubber powder; the frequency of ultrasonic wave cleaning is 180KHz, the ultrasonic wave cleaning time is 35min, the drying temperature during drying is 60℃, the drying time is 15min, and the rubber powder particle size is 200-300μm;
[0082] S3. Preparation of hydrogenated renewable materials:
[0083] The palm oil and potassium hydroxide were uniformly mixed in a mass ratio of 10:1, and then placed in a microwave reactor for heating reaction at a heating temperature of 150°C and a reaction time of 2 hours. After the reaction, pure water was added in a mass ratio of pure water to palm oil of 3:10, and stirred at a stirring speed of 100 r / min for 25 minutes, and then extracted to remove pure water to obtain a hydrogenated renewable material;
[0084] S4, raw material mixing:
[0085] Rubber powder, hydrogenated renewable materials, resorcinol, vulcanizing agent, accelerator, activator, and antioxidant are added into a mixer according to the weight portions in step S1 for mixing. The mixing time is 1.5 hours and the mixing speed is 160 rpm. After the mixing is completed, a mixture is obtained.
[0086] S5. Mixing:
[0087] The mixture obtained in step S4 is placed in a mixer for mixing at a mixing speed of 100 rpm, the temperature is raised to 100° C. at a heating rate of 7° C. / min, mixing is started, and the mixing time is 35 min. After the mixing is completed, a mixed material is obtained;
[0088] S6, calendering and cutting:
[0089] The mixture is put into a calender for calendering at a calendering temperature of 110°C. The mixture forms a sheet-like mixture under the pressure of the calender roller 36. The sheet-like mixture is air-cooled to 0°C. After cooling, the sheet-like mixture is cut to obtain a resorcinol rubber adhesive.
[0090] Embodiment 3:
[0091] like Figure 7 As shown, an optimized production process of resorcinol rubber adhesive comprises the following steps:
[0092] S1. Raw material preparation:
[0093] Take 50 parts of resorcinol, 80 parts of chloroprene rubber, 10 parts of hydrogenated renewable materials, 5 parts of vulcanizing agent, 3 parts of accelerator, 5 parts of activator, and 3 parts of antioxidant according to the following weight parts;
[0094] The vulcanizing agent is prepared by mixing ammonium sulfate and sodium hydrogen sulfide in a mass ratio of 1:1;
[0095] The accelerator is prepared by mixing zinc sulfate, phenylpropyl ketone and epoxy resin in a mass ratio of 1:2:1;
[0096] The active agent is prepared by mixing hydrogen peroxide and sodium thiosulfate in a mass ratio of 1:3;
[0097] The antioxidant is prepared by mixing catechol, dimethyl dithiocarboxylic acid and isobutyl diphenol in a mass ratio of 1:1:1;
[0098] S2. Rubber pretreatment:
[0099] The chloroprene rubber is cleaned by ultrasonic wave, and then crushed by a grinding device, and then dried to obtain rubber powder; the frequency of ultrasonic wave cleaning is 200KHz, the ultrasonic wave cleaning time is 40min, the drying temperature during the drying process is 80℃, the drying time is 20min, and the rubber powder particle size is 200-300μm;
[0100] S3. Preparation of hydrogenated renewable materials:
[0101] Palm oil and potassium hydroxide were mixed evenly at a mass ratio of 10:1, and then placed in a microwave reactor for heating reaction at a heating temperature of 200°C for 3 hours. After the reaction, pure water was added at a mass ratio of pure water to palm oil of 3:10. The mixture was stirred at a stirring speed of 120 r / min for 30 minutes, and then extracted to remove pure water to obtain a hydrogenated renewable material.
[0102] S4, raw material mixing:
[0103] Add rubber powder, hydrogenated renewable materials, resorcinol, vulcanizing agent, accelerator, activator, and antioxidant into a mixer according to the weight portions in step S1 for mixing. The mixing time is 2 hours and the mixing speed is 180 rpm. After the mixing is completed, a mixture is obtained.
[0104] S5. Mixing:
[0105] The mixture obtained in step S4 is placed in a mixer for mixing at a mixing speed of 120 rpm, the temperature is raised to 120° C. at a heating rate of 8° C. / min, mixing is started, and the mixing time is 40 min. After the mixing is completed, a mixed material is obtained;
[0106] S6, calendering and cutting:
[0107] The mixture is put into a calender for calendering at a calendering temperature of 120°C. The mixture forms a sheet-like mixture under the pressure of the calender roller 36. The sheet-like mixture is air-cooled to 5°C. After cooling, the sheet-like mixture is cut to obtain a resorcinol rubber adhesive.
[0108] Comparing Examples 1 to 3, the resorcinol rubber adhesive prepared in Example 3 has the best performance and the highest production efficiency, so Example 3 is the best example.
[0109] It should be noted that the grinding device, microwave reactor and calender used in Examples 1-3 are all products of the prior art, and those skilled in the art can select them according to their needs, which will not be elaborated here.
[0110] Example 4
[0111] On the basis of Example 3, Example 4 is different from Example 3 in that the grinding device in this embodiment has a different structure from the grinding device in Example 3, including a motor base 11, a grinding cylinder 12, a rotating motor 13, a rotating shaft 14, a short rod 15, a cutting cylinder 16, and a discharge port 17. The motor base 11 is fixedly connected to the grinding cylinder 12 through a fixed frame, the cutting cylinder 16 is fixedly connected above the grinding cylinder 12, the rotating motor 13 is fixedly connected inside the motor base 11, the lower end of the rotating shaft 14 is rotatably connected to the bottom of the grinding cylinder 12, and is drivingly connected to the output shaft of the rotating motor 13, the upper end of the rotating shaft 14 is rotatably connected to the top of the cutting cylinder 16 through the short rod 15, a grinding disc 18 is fixedly connected to the outer side of the bottom of the rotating shaft 14, two fixed plates 19 are fixedly connected above the rotating shaft 14, and a cutting stick 191 is rotatably connected on each side between the two fixed plates 19, and the discharge port 17 is fixedly connected to one side of the grinding cylinder 12.
[0112] Compared with Example 3, the grinding device provided in Example 4 can improve the efficiency of rubber grinding and further improve the production efficiency of rubber adhesive.
[0113] Example 5
[0114] On the basis of Example 4, Example 5 is different from Example 4 in that the microwave reactor in Example 5 includes a microwave generator 21, a microwave shell 22, a microwave chamber 23, a waveguide 24, a chamber door 25, a reaction tube 26, and a stirring frame 27. The microwave generator 21 is fixedly installed on the right side of the microwave shell 22, the microwave chamber 23 is located on the left side of the microwave shell 22, the microwave chamber 23 is connected to the microwave generator 21 through the waveguide 24, the chamber door 25 is hinged on the front side of the microwave chamber 23, the reaction tube 26 is placed inside the microwave chamber 23, the stirring frame 27 is fixedly connected to the top of the microwave shell 22 and is located above the microwave chamber 23, and two hydraulic rods 28 are fixedly connected to the top of the stirring frame 27, and the lower end of the hydraulic rod 28 is fixedly connected to a hydraulic plate 29, and the top of the hydraulic plate 29 is fixedly connected to a stirring motor 291, and the output shaft of the stirring motor 291 is transmission-connected to a stirring rod 292, and a sealing ring 293 is provided below the hydraulic plate 29.
[0115] Compared with Example 4, the microwave reactor provided in Example 5 can effectively improve the hydrogenation reaction of palm oil and improve the production efficiency of hydrogenated renewable materials.
[0116] Example 6
[0117] On the basis of Example 5, Example 6 differs from Example 5 in that the calender in Example 6 includes a pressing plate 31, a support frame 32, and a sliding frame 33. An electronic heating plate 311 is provided at the bottom of the pressing plate 31. The support frame 32 is fixedly connected to the bottom of the pressing plate 31. There are two sliding frames 33, which are respectively fixedly connected to the two sides of the support frame 32. A slider 34 is provided inside the sliding frame 33. The outer walls of the slider 34 on the front and rear sides are slidably connected to the sliding frame 33. An adjusting screw 35 is threadedly connected to the front and rear sides of the slider 34. The upper and lower ends of the adjusting screw 35 are rotatably connected to the upper and lower sides of the sliding frame 33 respectively. A roller 36 is rotatably connected between the two sliders 34. A calendering motor 37 is provided at one end of the roller. The calendering motor 37 is fixedly connected to the slider 34, and the output shaft of the calendering motor 37 is transmission-connected to the roller 36.
[0118] Compared with Example 5, the calender in Example 6 can keep the rubber adhesive softened during the calendering process, thereby improving the efficiency of rubber adhesive calendering, so Example 6 is the best example.
[0119] The rotating motor 13, microwave generator 21, stirring motor 291, calendering motor 37, and electronic heating plate 311 used in the above embodiments are all commercially available products. As long as they can achieve the functions of the present invention, those skilled in the art can choose to use them according to common sense, and no special limitations are made here.
Claims
1. An optimized production process for resorcinol rubber adhesive, characterized in that: The following steps are involved: S1. Raw material preparation: Take 20-50 parts of resorcinol, 50-80 parts of chloroprene rubber, 8-10 parts of hydrogenated renewable materials, 3-5 parts of vulcanizing agent, 1-3 parts of accelerator, 2-5 parts of active agent, and 1-3 parts of antioxidant according to the following weight parts; S2. Rubber pretreatment: The chloroprene rubber is cleaned by ultrasonic wave, and then crushed by grinding device, and then dried to obtain rubber powder; S3. Preparation of hydrogenated renewable materials: The palm oil and potassium hydroxide are uniformly mixed in a mass ratio of 10:1, and then placed in a microwave reactor for heating reaction at a heating temperature of 100-200°C and a reaction time of 1-3 hours. After the reaction, pure water is added in a mass ratio of pure water to palm oil of 3:10, and stirred at a stirring speed of 80-120 r / min for 20-30 minutes, and then extracted to remove pure water to obtain a hydrogenated renewable material; S4, raw material mixing: Add rubber powder, hydrogenated renewable materials, resorcinol, vulcanizing agent, accelerator, activator, and antioxidant into a mixer according to the weight portions described in step S1 for mixing. The mixing time is 1-2 hours and the mixing speed is 120-180 rpm. After the mixing is completed, a mixture is obtained. S5. Mixing: The mixture obtained in step S4 is placed in a mixer for mixing at a mixing speed of 60-120 rpm, the temperature is raised to 80-120° C. at a heating rate of 5-8° C. / min, mixing is started, and the mixing time is 30-40 min. After the mixing is completed, a mixed material is obtained; S6, calendering and cutting: The mixed material is placed in a calender for calendering at a calendering temperature of 100-120° C. The mixed material is formed into a sheet-like mixed material under the pressure of the roller (36) of the calender, and the sheet-like mixed material is air-cooled to -3-5° C. After the cooling is completed, the sheet-like mixed material is cut to obtain a resorcinol rubber adhesive; The vulcanizing agent is prepared by mixing ammonium sulfate and sodium hydrogen sulfide in a mass ratio of 1:1; The accelerator is prepared by mixing zinc sulfate, phenylpropyl ketone and epoxy resin in a mass ratio of 1:2:1; The active agent is prepared by mixing hydrogen peroxide and sodium thiosulfate in a mass ratio of 1:3; The antioxidant is prepared by mixing catechol, dimethyl dithiocarboxylic acid and isobutyl diphenol in a mass ratio of 1:1:1; The frequency of ultrasonic cleaning in step S2 is 150-200KHz, the ultrasonic cleaning time is 30-40min, the drying temperature during the drying process is 50-80°C, and the drying time is 10-20min; The rubber powder in step S2 has a particle size of 200-300 μm; The grinding device comprises a motor base (11), a grinding cylinder (12), a rotating motor (13), a rotating shaft (14), a short rod (15), a cutting cylinder (16), and a discharge port (17). The motor base (11) is fixedly connected to the grinding cylinder (12) via a fixed frame, the cutting cylinder (16) is fixedly connected above the grinding cylinder (12), the rotating motor (13) is fixedly connected inside the motor base (11), the lower end of the rotating shaft (14) is rotatably connected to the bottom of the grinding cylinder (12), and is drivingly connected to the output shaft of the rotating motor (13), the upper end of the rotating shaft (14) is rotatably connected to the top of the cutting cylinder (16) via the short rod (15), a grinding disc (18) is fixedly connected to the outer side of the bottom of the rotating shaft (14), two fixed plates (19) are fixedly connected above the rotating shaft (14), and a cutting rod (191) is rotatably connected to each of the two sides between the two fixed plates (19), and the discharge port (17) is fixedly connected to one side of the grinding cylinder (12); The microwave reactor comprises a microwave generator (21), a microwave shell (22), a microwave chamber (23), a waveguide (24), a chamber door (25), a reaction tube (26), and a stirring frame (27). The microwave generator (21) is fixedly mounted on the right side of the microwave shell (22); the microwave chamber (23) is located on the left side of the microwave shell (22); the microwave chamber (23) and the microwave generator (21) are connected via the waveguide (24); the chamber door (25) is hinged on the front side of the microwave chamber (23); and the reaction tube (26) is provided on the stirring frame (27). 26) is placed inside the microwave chamber (23), the stirring frame (27) is fixedly connected to the top of the microwave shell (22) and is located above the microwave chamber (23), the top of the stirring frame (27) is fixedly connected to two hydraulic rods (28), the lower ends of the hydraulic rods (28) are fixedly connected to a hydraulic plate (29), the top of the hydraulic plate (29) is fixedly connected to a stirring motor (291), the output shaft of the stirring motor (291) is transmission-connected to a stirring rod (292), and a sealing ring (293) is provided below the hydraulic plate (29).