Glass fiber and glass fiber composition

By using glass compositions with high MgO content in glass fibers, combining the ratio of SiO2, Al2O3 and alkali metal oxides, the spinning difficulties are solved, and glass fiber production with high Young's modulus and small diameter is achieved. Suitable for FRP and other materials.

CN116390896BActive Publication Date: 2024-11-08NIPPON SHEET GLASS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280006762.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-05-31
Filing Date
2022-08-04
Publication Date
2024-11-08
Estimated Expiration
2042-08-04

AI Technical Summary

Technical Problem

The prior art is difficult to spin glass fibers with small fiber diameters, and high Mg glasses are prone to devitrification when spinning with small diameters, resulting in manufacturing difficulties.

Method used

Using a glass composition with an MgO content of more than 15%, combined with the ratio of SiO2, Al2O3 and alkali metal oxides, the viscosity logη at the devitrification temperature is controlled to be more than 2.6, to ensure that the fiber diameter is less than 18 μm, and by adjusting the Na2O ratio and CaO content to improve spinning properties.

Benefits of technology

The production of glass fibers with high Young's modulus and small diameter is achieved. They are suitable for thin reinforced materials such as FRP, and the fiber diameter can be as thin as 7 to 15 μm to maintain high reinforcement capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004156462540000021
    Figure BDA0004156462540000021
  • Figure BDA0004156462540000022
    Figure BDA0004156462540000022
  • Figure BDA0004156462540000091
    Figure BDA0004156462540000091
Patent Text Reader

Abstract

The present invention provides a glass fiber having a fiber diameter of 18 μm or less, the glass fiber comprising a glass composition, the content of MgO in the glass composition being 15 mol% or more, and the common logarithm logη of the viscosity η [dPa·s] of the glass composition at the devitrification temperature being 2.6 or more. In addition, a glass composition is provided, wherein, expressed in mol%, it comprises: SiO2: 50 to 65%, Al2O3: 5 to 26%, B2O3: 0 to 1.6%, MgO: 15 to 30%, CaO: 0 to 8%, Li2O: 0 to 2.4%, Na2O: greater than 0.2% and less than 2.85%, the total content of Li2O, Na2O and K2O being 0.3 to 3.0% or less, and the ratio of the content of Na2O to the total being 0.2 or more and 0.95 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to glass fibers and glass compositions suitable for glass fibers. Background Art

[0002] Most of the glass fibers for practical use are composed of glass compositions whose Young's modulus is 90 GPa or less. However, glass compositions whose Young's modulus exceeds 90 GPa are also known. For example, Patent Document 1 discloses a glass composition containing a large amount of rare earth oxides. The total content of Y2O3 and La2O3 in the glass composition of Patent Document 1 is in the range of 20 to 60 weight %. However, if the content of rare earth oxides is high, the manufacturing cost increases. Taking this into consideration, Patent Document 2 discloses a technology for increasing the Young's modulus of a glass composition without requiring a large amount of rare earth oxides. In the glass composition of Patent Document 2, as a component for increasing the Young's modulus, 15 to 30% of MgO expressed in mole % is contained.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: International Publication No. 2006 / 057405

[0006] Patent Document 2: Japanese Patent No. 6391875 Summary of the invention

[0007] Problems to be solved by the invention

[0008] It is difficult to spin a glass composition containing 15 mol% or more of MgO as a component that increases the Young's modulus (referred to as "high Mg glass" in this paragraph) into glass fibers with a small fiber diameter. Even with high Mg glass that can be spun into glass fibers with a relatively large fiber diameter, manufacturing problems will frequently occur if the fiber diameter is reduced. High Mg glass is prone to devitrification in a nozzle used to spin glass fibers with a small diameter. Therefore, an object of the present invention is to provide a new glass fiber with a high Young's modulus and a relatively small diameter. Another object of the present invention is to provide a glass composition suitable for glass fibers with a high Young's modulus and a relatively small diameter.

[0009] Means used to solve problems

[0010] The present inventors have repeatedly studied the mechanism of devitrification when spinning a glass composition having a high MgO content, and have completed the present invention.

[0011] The present invention provides a glass fiber having a fiber diameter of 18 μm or less.

[0012] The glass fiber includes a glass composition, wherein the content of MgO in the glass composition expressed in mol% is 15% or more, and the common logarithm logη of the viscosity η [dPa·s] of the glass composition at the devitrification temperature is 2.6 or more.

[0013] From another aspect, the present invention provides a glass composition for glass fiber, wherein:

[0014] In mole % it contains:

[0015]

[0016] The total content of Li2O, Na2O and K2O is 0.3 to 3.0% or less.

[0017] The Na2O ratio determined from the ratio of the Na2O content to the total content of Li2O, Na2O, and K2O is 0.2 or more and 0.95 or less.

[0018] From another aspect, the present invention provides a glass composition for glass fiber, wherein:

[0019] In mole % it contains:

[0020]

[0021] The common logarithm value logη of the viscosity η [dPa·s] at the devitrification temperature is 2.6 or more.

[0022] From another aspect, the present invention provides a glass composition for glass fiber, wherein the Young's modulus is greater than 93 GPa, wherein:

[0023] Expressed in mole %,

[0024] The total content of Li2O, Na2O and K2O is 0.3 to 3.0% or less.

[0025] The Na2O ratio determined from the ratio of the Na2O content to the total content of Li2O, Na2O, and K2O is 0.2 or more and 0.95 or less.

[0026] Effects of the Invention

[0027] According to the present invention, there is provided a novel glass fiber having a high Young's modulus and a relatively small diameter. According to the present invention, there is provided a novel glass composition suitable for a glass fiber having a high Young's modulus and a relatively small diameter. DETAILED DESCRIPTION

[0028] Hereinafter, embodiments of the present invention will be described, but the following description is not intended to limit the present invention to a specific embodiment. In this specification, the contents of the components of the following glass compositions are all expressed in mol%, and mol% is basically expressed as "%". In this specification, "substantially not containing" and "substantially not containing" mean that the content is less than 0.1 mol%, less than 0.05 mol%, less than 0.01 mol%, less than 0.005 mol%, and further less than 0.003 mol%, and depending on the situation, less than 0.001 mol%. The meaning of "substantially" is that trace amounts of impurities derived from glass raw materials, manufacturing equipment, etc. are allowed to be contained. "Alkali metal oxides" refer to Li2O, Na2O, and K2O, and are sometimes described as R2O. The upper and lower limits of the contents described below can be arbitrarily combined.

[0029] [Fiberglass]

[0030] In one embodiment of the present invention, the fiber diameter of the glass fiber is 18 μm or less. The glass fiber comprises a glass composition, wherein the content of MgO in the glass composition is 15% or more, and the common logarithm value logη of the viscosity η [dPa·s] at the devitrification temperature of the glass composition is 2.6 or more. An example of the glass composition will be described later.

[0031] In another embodiment of the present invention, the glass fiber includes a glass composition described below. The fiber diameter of the glass fiber may be 18 μm or less.

[0032] The fiber diameter of the glass fibers of these embodiments (hereinafter referred to as "glass fibers of the present embodiment") can be 15 μm or less, 13 μm or less, 11 μm or less, 10 μm or less, 9 μm or less, and further 7 μm or less. The glass fibers of the present embodiment can have a high Young's modulus, and therefore can exhibit a high reinforcing ability even if the diameter is reduced. Therefore, the glass fibers of the present embodiment are particularly suitable for thin reinforced materials, such as thin glass fiber reinforced plastics (FRP). However, the objects for which the glass fibers of the present embodiment are used are not limited to FRP, and there is no restriction on the thickness of the objects. The lower limit of the fiber diameter of the glass fibers of the present embodiment is not particularly limited, and can be 3 μm or more, and further 7 μm or more. The glass fibers of the present embodiment can have a high Young's modulus and a thin diameter, or can have a diameter in a range that is not too thin, such as a diameter in the range of 7 to 15 μm, and further 9 to 13 μm.

[0033] The glass fiber of the present embodiment may include a glass composition and components such as various known treatment agents and resins appropriately added according to the application.

[0034] [Glass composition]

[0035] <ingredients>

[0036] Hereinafter, each component that can constitute the glass composition will be described.

[0037] (SiO2)

[0038] SiO2 is a component that forms the skeleton of glass, and is also a component that adjusts the devitrification temperature and viscosity when forming glass and improves acid resistance. The content of SiO2 is, for example, 50 to 65%. The lower limit of the content of SiO2 is, for example, 52% or more, 54% or more, 55% or more, 56% or more, 57% or more, 57.5% or more, and depending on the situation, 58% or more, and further 59% or more. The upper limit of the content of SiO2 is, for example, 63% or less, 62% or less, and depending on the situation, 61% or less.

[0039] (Al2O3)

[0040] Al2O3 is a component that adjusts the devitrification temperature and viscosity when forming glass and improves the water resistance of glass. The content of Al2O3 is, for example, 5 to 26%. The lower limit of the content of Al2O3 is, for example, 7.5% or more, 8% or more, 9% or more, 10% or more, 10.5% or more, 11% or more, 12% or more, and depending on the situation, 12.5% ​​or more, and further 13% or more. The upper limit of the content of Al2O3 is, for example, 20% or less, 18% or less, 17.5% or less, 16% or less, and depending on the situation, 15% or less.

[0041] (MgO)

[0042] MgO is a component that contributes to the improvement of Young's modulus and affects the devitrification temperature, viscosity, etc. The content of MgO is, for example, 15 to 30%. The lower limit of the content of MgO is, for example, 16% or more, 17.5% or more, 18% or more, 20% or more, 22% or more, and depending on the situation, 23% or more, and further 24% or more. The upper limit of the content of MgO is, for example, 27% or less, 26% or less, and depending on the situation, 25% or less.

[0043] The contents of SiO 2 , Al 2 O 3 , and MgO are as described above. The upper and lower limits described above can be set by arbitrarily combining them, but the desired ranges are as follows.

[0044] Example 1 SiO2: 52-62% and Al2O3: 7.5-26%

[0045] Example 2 In Example 1, Al2O3: 9-26%

[0046] Example 3 In Example 2, SiO2: 55-62%

[0047] Al2O3: 10.5~17.5%

[0048] MgO: 17.5~30%

[0049] Example 4 In Example 3, Al2O3: 11-17.5%

[0050] MgO: 20-30%

[0051] However, the above are merely examples, and the content of each component may be set without being limited to Examples 1 to 4.

[0052] SiO2, Al2O3, and MgO are important components for forming a glass composition having a high Young's modulus and being practical. The total content of these components exceeds 90%, and may be 91% or more, and further 92% or more. The total content of SiO2, Al2O3, and MgO may be, for example, 98.5% or less, and further 98% or less. If the total content is suppressed to this extent, there is more room for adjusting the characteristics by adding other components.

[0053] The glass composition of this embodiment preferably further contains CaO and / or alkali metal oxides. A glass composition with a high MgO content tends to have a viscosity η at a devitrification temperature that is too low. However, the viscosity can be adjusted by adding CaO and alkali metal oxides. The total content of CaO and alkali metal oxides is, for example, 0.1% or more, 0.5% or more, 1.0% or more, or 1.5% or more.

[0054] (CaO)

[0055] CaO is a component that adjusts the devitrification temperature and viscosity when forming glass. The content of CaO is, for example, 0 to 8%. The lower limit of the content of CaO is, for example, 0.1% or more, 0.5% or more, 0.7% or more, 1% or more, and depending on the situation, 2% or more, and further 3% or more. The upper limit of the content of CaO is, for example, 6% or less, 5.5% or less, 5% or less, and further 4% or less.

[0056] (Alkali Metal Oxides)

[0057] Alkali metal oxides (R2O) are components that adjust the devitrification temperature and viscosity when forming glass. The total content of alkali metal oxides, specifically Li2O+Na2O+K2O, is, for example, 0.3 to 3.0%. The lower limit of the content of alkali metal oxides is, for example, 0.5% or more, 0.7% or more, and further 0.8% or more, and depending on the situation, 1.0% or more. The upper limit of the content of alkali metal oxides is, for example, 2.5% or less, 2.0% or less, 1.8% or less, 1.5% or less, and depending on the situation, less than 1.1%. When the content of alkali metal oxides is high, there is a situation where the Young's modulus cannot be fully increased.

[0058] The content of Na2O is, for example, greater than 0.2% and less than 3%, or, for example, greater than 0.2% and less than 2.85%. The lower limit of the content of Na2O is, for example, greater than 0.25%, greater than 0.3%, greater than 0.4%, and further greater than 0.5%. The upper limit of the content of Na2O is, for example, less than 2.5%, less than 2.0%, less than 1.5%, less than 1.0%, less than 0.8%, and depending on the circumstances, less than 0.6%, and further less than 0.55%.

[0059] It is not necessary to contain both Li2O and K2O, but it is preferable to contain at least one of them. The total content of Li2O and K2O is preferably 0.1% or more.

[0060] The content of Li2O is, for example, 0 to 3%, or, for example, 0 to 2.4%. The lower limit of the content of Li2O is, for example, 0.1% or more, 0.2% or more, and depending on the situation, 0.3% or more. The upper limit of the content of Li2O is, for example, 2.0% or less, 1.5% or less, 1.0% or less, 0.8% or less, and depending on the situation, 0.6% or less, 0.5% or less, and further 0.4% or less. A preferred example of the content of Li2O is 0.1 to 0.8%.

[0061] Li2O is more advantageous than Na2O and K2O in adjusting the devitrification temperature and other characteristics while suppressing the influence of reducing the Young's modulus. Therefore, when adding, for example, 0.3% or more of an alkali oxide to a glass composition in order to achieve a high Young's modulus, the content of Li2O is usually adjusted to be higher than the content of Na2O and the content of K2O. For example, in each example of Patent Document 2, when the content of the alkali metal oxide is 0.3% or more, Li2O is added so that its content is 0.45% or more higher than the content of Na2O and the content of K2O.

[0062] However, in order to effectively control the viscosity at the devitrification temperature, it is desirable to give priority to the appropriate control of the Na2O ratio described later. In addition, Li2O is relatively expensive as a raw material among alkali metal oxides. In consideration of these aspects, the content of Li2O may include a trace amount within a range not higher than the content obtained by adding 2% to the content of Na2O. The content of Li2O may also include a trace amount within a range not exceeding the content of Na2O.

[0063] The content of K2O is, for example, 0 to 2.4%. The lower limit of the content of K2O is, for example, 0.01% or more, further 0.02% or more, and depending on the situation, 0.05% or more. The upper limit of the content of K2O is, for example, 1.0% or less, 0.5% or less, 0.2% or less, and depending on the situation, 0.1% or less. K2O has a greater effect on reducing the Young's modulus than Li2O and Na2O. The content of K2O is preferably suppressed to be less than the content of Li2O and the content of Na2O. K2O may be substantially absent.

[0064] The relative size relationship of the alkali metal oxides shown in the above two paragraphs can be expressed as follows, where [Li2O] represents the content rate (mol %) of Li2O, [Na2O] represents the content rate (mol %) of Na2O, and [K2O] represents the content rate (mol %) of K2O. The alkali metal oxide is preferably contained in a manner that satisfies at least one of the following formulae.

[0065] 0<[Li2O]≤([Na2O]+2)

[0066] 0<[Li2O]≤[Na2O]

[0067] [K2O]<[Na2O]

[0068] [K2O]<[Li2O]

[0069] When the total content of R2O is greater than 0.3%, more specifically in the range of 0.3 to 3.0%, the ratio of the content of Na2O to the content of R2O ([R2O] / [Na2O] according to the above-mentioned recording method, hereinafter also referred to as "Na2O ratio") is preferably greater than 0.2 and less than 0.95. If the Na2O ratio is adjusted to an appropriate range, the spinnability of the glass composition with a high MgO content is improved. The lower limit of the Na2O ratio may be, for example, greater than 0.22, greater than 0.27, and further greater than 0.3. The upper limit of the Na2O ratio may be, for example, less than 0.92, less than 0.86, less than 0.8, less than 0.78, less than 0.73, and less than 0.7 depending on the circumstances. If the Na2O ratio is appropriately adjusted, the desired effect, such as a sufficient increase in logη, can be obtained by adding a limited amount of alkali metal oxide.

[0070] That is, when the content (mol %) of the alkali metal oxide is preferably represented by [R2O], the following relationship is established.

[0071] 0.3≤[R2O]≤3.0

[0072] 0.2≤([Na2O] / [R2O])≤0.95

[0073] (B2O3)

[0074] B2O3 is a component that forms the skeleton of glass, and is also a component that adjusts the devitrification temperature and viscosity when forming glass. The content of B2O3 is, for example, 0 to 1.6%. The lower limit of the content of B2O3 is, for example, 0.1% or more, 0.5% or more, or 1.0% or more depending on the situation. The upper limit of the content of B2O3 is, for example, less than 1.5%, or less than 1.2% depending on the situation. B2O3 may be substantially absent.

[0075] (Y2O3 and La2O3)

[0076] Y2O3 and La2O3 are components that contribute to the improvement of Young's modulus. However, the raw materials of these components are relatively expensive. The total content of Y2O3 and La2O3 is, for example, 0 to 0.5%, and further 0 to 0.3%. The upper limit of the total content of Y2O3 and La2O3 can be 0.1% or less. Y2O3 and La2O3 can be substantially free of each other.

[0077] (Other ingredients)

[0078] The glass composition may also contain components other than those mentioned above. As other components that the glass composition may contain, SrO, BaO, ZnO, TiO2, ZrO2, Fe2O3, Cl2, F2, SnO2, CeO2, P2O5, SO3 can be exemplified. The content of these components is, for example, 0 to 5%, respectively. The upper limit of this content may be 3% or less, 1% or less, and further 0.5% or less. Other components, that is, components other than the above-mentioned SiO2 to La2O3 components, may be substantially absent. The total content of other components may be 7% or less, 5% or less, and further 3% or less. It should be noted that the content of components that can take multiple valences in the glass composition is calculated by converting them into oxides of the valences shown above according to conventional methods. For example, a portion of iron oxide may exist in the glass composition in the form of FeO, but its content is converted into Fe2O3 and expressed.

[0079] <Features>

[0080] In one embodiment of the present invention, the common logarithm of the viscosity η of the glass composition at the devitrification temperature is, for example, 2.6 or more. The unit of η is [dPa·s]. In addition, the present invention includes a technique for improving a glass composition having a Young's modulus of, for example, 93 GPa or more. The following describes logη and Young's modulus.

[0081] (logη)

[0082] It has been found that a glass composition with high logη is suitable for spinning glass fibers with relatively small fiber diameters. For example, logη is 2.6 or more. The lower limit of logη may be 2.7 or more, 2.8 or more, 2.9 or more, 2.93 or more, and may be 3.0 or more depending on the situation. The upper limit of logη is not particularly limited, and is, for example, 3.4 or less, and further, 3.2 or less.

[0083] Glass compositions with a high MgO content and suitable for improving Young's modulus tend to have a smaller difference between the operating temperature suitable for spinning and the devitrification temperature. Glass compositions with a small difference between the two temperatures are generally difficult to spin, and are particularly difficult to spin for glass fibers with small fiber diameters. However, such difficulty in spinning can be alleviated by controlling logη.

[0084] (Young's modulus)

[0085] The Young's modulus of the glass composition is, for example, 93 GPa or more. The lower limit of the Young's modulus is 95 GPa or more, 97 GPa or more, 99 GPa or more, and in some cases, 100 GPa or more. The upper limit of the Young's modulus is not particularly limited, and is, for example, 115 GPa or less, and further, 110 GPa or less.

[0086] <Examples of Glass Compositions>

[0087] In one embodiment of the present invention, the glass composition comprises:

[0088]

[0089] The total content of Li2O, Na2O and K2O is 0.3 to 3.0% or less, and the ratio of the content of Na2O to the total content of Li2O, Na2O and K2O is 0.2 to 0.95 or less.

[0090] In another embodiment of the present invention, the glass composition comprises:

[0091]

[0092] logη is greater than 2.6.

[0093] In another embodiment of the present invention, the glass composition has a Young's modulus of 93 GPa or more, wherein:

[0094] The total content of Li2O, Na2O and K2O is 0.3 to 3.0% or less, and the ratio of the content of Na2O to the total content of Li2O, Na2O and K2O is 0.2 to 0.95 or less.

[0095] In another embodiment of the present invention, in the glass composition,

[0096] The total content of SiO2, Al2O3 and MgO expressed in mol% exceeds 90%,

[0097] The common logarithm value logη of the viscosity η [dPa·s] at the devitrification temperature is 2.6 or more.

[0098] The above descriptions of the components and properties are all applicable to the glass compositions in each form exemplified above.

[0099] The glass compositions in the above-mentioned forms are suitable for the manufacture of glass fibers, especially glass fibers whose fiber diameters reach the above-mentioned range. In one embodiment of the present invention, the glass fibers contain the glass compositions in the above-mentioned forms, or are composed of the glass compositions in the above-mentioned forms. The glass fibers may be, for example, in a form that conforms to at least one selected from bundled yarns, rovings, spinnings, cloths, chopped strands, glass wool, and milled fibers. Cloths are, for example, roving cloths and spinning cloths. However, the glass compositions in the above-mentioned forms can also be used in the form of glass molded bodies other than glass fibers due to their excellent properties. An example of a glass molded body is granular glass. Granular glass can be manufactured by breaking glass fibers; or it can be manufactured using a nozzle corresponding to the target shape in the same manner as glass fibers. Therefore, the glass compositions in the above-mentioned forms are also suitable for manufacturing granular glass while avoiding devitrification. In one embodiment of the present invention, the granular glass contains the glass compositions in the above-mentioned forms, or is composed of the glass compositions in the above-mentioned forms.

[0100] The granular glass may be, for example, at least one selected from the group consisting of flaky glass, glass powder, glass beads, and fine flakes. The granular glass may also be used for FRP, that is, for reinforcing a body to be reinforced, such as a resin.

[0101] [Non-woven fabrics, rubber reinforcing wire]

[0102] Each glass fiber provided by the present invention can be used for the same purpose as the existing glass fiber. According to one embodiment of the present invention, a glass fiber nonwoven fabric containing glass fibers is provided. In addition, according to one embodiment of the present invention, a rubber reinforcing wire material containing a bundled yarn formed by bundling glass fibers is provided. The glass fiber can also be used for other purposes. Other uses include the reinforcement of a reinforced body represented by a resin.

[0103] Example

[0104] Hereinafter, the embodiment of the present invention will be described in more detail by way of examples and comparative examples. In addition, in Tables 1 to 3, the content ratios of the compositions are also expressed in mol %.

[0105] <Glass Compositions A to H and W to Z>

[0106] Common glass raw materials such as silica sand are prepared in the form of the compositions shown in Table 1, and the batch materials of the glass raw materials are respectively prepared in the examples and comparative examples. Using an electric furnace, each batch material is heated to 1500-1600°C to melt it, and this state is maintained for about 4 hours until the composition becomes uniform. Then, a part of the molten glass (glass melt) is flowed onto an iron plate, and slowly cooled to room temperature in an electric furnace to obtain a glass composition (plate-like object, glass sample) in the form of a block. For these glass compositions, the characteristics are evaluated as described below. The results are shown in Table 1.

[0107] (Devitrification temperature)

[0108] The glass composition crushed to a particle size of 1.0 to 2.8 mm is placed in a platinum boat and kept in an electric furnace with a temperature gradient (800 to 1400°C) for 2 hours. The devitrification temperature is calculated based on the maximum temperature of the electric furnace corresponding to the position where the crystal appears. In the case where the glass becomes turbid and crystals cannot be observed, the maximum temperature of the electric furnace corresponding to the position where the turbidity appears is taken as the devitrification temperature. Here, the particle size is a value measured by a sieving method. It should be noted that the temperature (temperature distribution in the electric furnace) that varies depending on the location in the electric furnace is pre-determined, and the glass composition placed in a specified location in the electric furnace is heated at the pre-determined temperature of the specified location.

[0109] (Viscosity at devitrification temperature)

[0110] The viscosity η of the obtained glass composition at the devitrification temperature was measured by a common platinum ball pulling method, and logη was calculated from the measured value.

[0111] (Young's modulus)

[0112] The Young's modulus is calculated by measuring the longitudinal wave velocity vl and the transverse wave velocity vt of elastic waves propagating in the glass by a conventional ultrasonic method, and using the density ρ of the glass measured separately by the Archimedean method, E=3p·v t 2 ·(v1 2 -4 / 3·v t 2 ) / (v1 2 -v t 2 ) formula to find out.

[0113] <Spinning Test>

[0114] For each glass composition having compositions A to E and W to Z, a spinning test was performed in which a melt was spun using a platinum nozzle.

[0115] The results of the spinning test were evaluated based on the following criteria.

[0116] ○: Stable spinning suitable for production can be performed for a long time.

[0117] △: Spinning can be performed for 10 minutes or more, but long-term stable spinning cannot be achieved.

[0118] ×1: The platinum nozzle used was clogged due to devitrification.

[0119] ×2: The viscosity of the molten glass is too low to allow spinning.

[0120] <Adjustment of Alkali Metal Oxide>

[0121] Glass compositions were prepared in the same manner as above with respect to compositions C1 to C2 and compositions D1 to D4 in which only the content of alkali metal oxides was changed, respectively, using compositions C and D as references, and their properties were evaluated.

[0122] As shown in Table 2, it can be confirmed that the logη of compositions W and X is small and is not suitable for spinning with a fiber diameter of less than 18μm. For compositions Y and Z, spinning itself cannot be carried out. In contrast, for compositions A to E with logη of more than 2.6, it was confirmed that even fibers with small diameters can be spun well. As shown in Table 3, the closer the Na2O ratio (molar ratio Na2O / R2O) is to about 0.5, the larger the logη. It is believed that the appropriate Na2O ratio to achieve logη of more than 2.6 is 0.2 to 0.95, and further 0.2 to 0.8. However, according to composition W in Table 1, it can be confirmed that in a composition with too little content of alkali metal oxide R2O, even if the Na2O ratio is adjusted, the contribution to the increase in logη is not large. It should be noted that the Young's modulus of compositions A to H is slightly lower than that of compositions W to Z, but is large enough for general glass fiber compositions.

[0123] The operating temperatures of glasses A to H are in the range of 1268 to 1356° C. The difference between the operating temperature and the devitrification temperature of glasses A to H is less than 60° C. This also applies to glasses D2 to D4. The operating temperature is a temperature at which logη becomes 3.0.

[0124] [Table 1]

[0125]

[0126] [Table 2]

[0127]

[0128] × 1: Blockage due to devitrification × 2: Unable to form a thread

[0129] [Table 3]

[0130]

Claims

1. A glass composition for glass fiber, in, In mole % it contains: Not. 2 50%~65%, <h2 style=";text-align:left;direction:ltr">Al<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> O<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 5%~26% B 2 O 3 0%~1.6%、 MgO 20%~30%, CaO 0%~6%, Li 2 0.1%~0.8%, So 2 0.25%~2.85%, Li 2 O、Na 2 O and K 2 The total content of O is 0.5% to 3.0%. According to Na 2 O content relative to Li 2 O、Na 2 O and K 2 The total ratio of O content to Na 2 O ratio is 0.3 or more and 0.7 or less, Y 2 O 3 La 2 O 3 The total content of is 0% to 0.5%.

2. The glass composition according to claim 1, in, SiO 2 、Al 2 O 3 The total content of O and MgO expressed in mol % exceeds 90%.

3. The glass composition according to claim 1, in, B expressed in mol% 2 O 3 The content rate is 0.1% to 1.6%.

4. The glass composition according to claim 3, in, SiO in mol% 2 The content rate is 57% to 62%.

5. The glass composition according to claim 1, in, SiO in mol% 2 The content rate is 52% to 62%, Al in mol% 2 O 3 The content rate is 7.5% to 26%.

6. The glass composition according to claim 5, in, Al in mol% 2 O 3 The content rate is 9% to 26%.

7. The glass composition according to claim 6, in, Expressed in mole %, SiO 2 The content rate is 55% to 62%, Al 2 O 3 The content rate is 10.5% to 17.5%.

8. The glass composition according to claim 7, in, Expressed in mole %, Al 2 O 3 The content rate is 11% to 17.5%.

9. The glass composition according to claim 1, in, Contains virtually no Y 2 O 3 .

10. The glass composition according to claim 1, in, The common logarithm value of the viscosity η at the devitrification temperature is 2.6 or more, The unit of viscosity η is dPa·s. The Young's modulus is 99 GPa or more.

11. A glass composition for glass fiber, in, In mole % it contains: According to Na 2 O content relative to Li 2 O、Na 2 O and K 2 The total ratio of O content to Na 2 O ratio is 0.3 or more and 0.7 or less, The common logarithm value of the viscosity η at the devitrification temperature is 2.9 or more, The unit of viscosity η is dPa·s. The Young's modulus is 99 GPa or more.

12. The glass composition according to claim 11, in, The logη is greater than or equal to 2.

93.

13. The glass composition according to claim 11, in, Contains virtually no Y 2 O 3 . 14 . A glass fiber comprising the glass composition according to claim 1 .

15. The glass fiber according to claim 14, in, The fiber diameter is 18 μm or less.

16. The glass fiber according to claim 14, in, The fiber has a form that conforms to at least one selected from the group consisting of bundled yarn, roving, spun yarn, cloth, chopped strands, glass wool, and milled fiber.

17. A rubber reinforcing wire material comprising a bundled yarn formed by bundling the glass fibers according to claim 14.

18. A glass fiber nonwoven fabric comprising the glass fiber according to claim 14.

19. A particulate glass comprising a glass composition, The glass composition comprises, expressed in mol %, Li 2 O、Na 2 O and K 2 The total content of O is 0.5% to 3.0%. According to Na 2 O content relative to Li 2 O、Na 2 O and K 2 The total ratio of O content to Na 2 O ratio is 0.3 or more and 0.7 or less, Y 2 O 3 La 2 O 3 The total content of is 0% to 0.5%.

20. A particulate glass comprising a glass composition, The glass composition comprises, expressed in mol %, According to Na 2 O content relative to Li 2 O、Na 2 O and K 2 The total ratio of O content to Na 2 O ratio is 0.3 or more and 0.7 or less, The common logarithm value logη of the viscosity η of the glass composition at the devitrification temperature is 2.9 or more, in, The unit of viscosity η is dPa·s. The Young's modulus is 99 GPa or more.