A preparation process of matt homogeneous glass

By using the masking film process in the preparation of matte one-piece glass, the problems of long process flow and low production capacity of exposure and development technology have been solved, and efficient and beautiful production of matte one-piece glass has been achieved, improving production capacity and product quality.

CN116395973BActive Publication Date: 2024-10-18合肥金龙浩科技有限公司
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310350660.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-18
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

In the existing matte one-piece glass preparation process, the exposure and development technology process is long and the production capacity is low. For 3D glass with high curvature, there are insufficient exposure and ink curing problems, which affects the matte effect.

Method used

Using the masking film process, by attaching the masking film to the glass, the preset glossy area is exposed, spraying acid-resistant ink, and performing surface drying, baking, cleaning, AG etching, ink removal, and polishing to simplify the process and increase production capacity. , and use high-temperature-resistant masking film to ensure that the matte junction is neatly distinguished and looks beautiful.

Benefits of technology

It achieves low cost, high productivity, and easy operation. The masking film has good high temperature resistance and adhesion, avoids the phenomenon of warping of the masking film and residual glue, and improves the preparation efficiency and product quality of matte one-piece glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116395973B_ABST
    Figure CN116395973B_ABST
Patent Text Reader

Abstract

The present invention discloses a process for preparing matt homogeneous glass, comprising the following steps: taking glass, one side of the glass comprising a preset glossy area and a preset matt area, attaching a shielding film on the glass so that the preset glossy area is exposed, spraying acid-resistant ink on the preset glossy area, and then sequentially performing surface drying, baking, film tearing, cleaning, AG etching, ink removal, and polishing to obtain matt homogeneous glass. The process of the present invention has low cost, high production capacity, and simple operation. The shielding film used has good high temperature resistance and strong adhesion. After surface drying and baking, the shielding film has no warping phenomenon, and there is no residual glue phenomenon when the film is torn, so that the interface between matt and gloss can be neatly distinguished and has a beautiful appearance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass, and in particular to a preparation process of matte homogeneous glass. Background Art

[0002] There are both glossy and etched matte surfaces (matte) on the same glass. This kind of glass is called glossy and matte homogeneous glass. The existing method for preparing glossy and matte homogeneous glass is generally exposure and development technology. The process flow is: first spray the entire surface of the glass with exposure and development ink, then locally expose and UV cure the position that needs to be protected, and then clean the oil film in other areas that has not been UV cured (referred to as development), and then bake, clean, strong acid etch, de-ink, and chemical polish to obtain glossy and matte homogeneous glass.

[0003] The process flow of exposure and development technology is relatively long; the production capacity of the exposure machine is relatively low, with a single machine capacity of 1500 pcs / day; and for 3D glass with a higher curvature, due to the height difference, there is insufficient exposure at the edge of the arc, and the ink cannot be completely cured, which will cause the subsequent ink to be easily washed away, losing the function of protecting the local area, and thus affecting the matte effect of the glass. Summary of the invention

[0004] Based on the technical problems existing in the background technology, the present invention proposes a preparation process of matte homologous glass. The process of the present invention has low cost, high production capacity, and easy operation. The shielding film used has good high temperature resistance and strong adhesion. After surface drying and baking, the shielding film has no warping phenomenon, and there is no residual glue when the film is torn off, so that the interface between matte and light can be neatly distinguished and the appearance is beautiful.

[0005] The present invention proposes a preparation process of matte homogeneous glass, comprising the following steps: taking glass, one side of the glass comprising a preset glossy area and a preset matte area, attaching a shielding film on the glass so that the preset glossy area is exposed, then spraying acid-resistant ink on the preset glossy area, and then sequentially performing surface drying, baking, film tearing, cleaning, AG etching, ink removal, and polishing to obtain the matte homogeneous glass.

[0006] Preferably, the preset matte area of ​​the glass is completely covered by the masking film.

[0007] When the preset matte area of ​​the glass is completely covered by the masking film, acid-resistant ink can be sprayed on the preset glossy area to save acid-resistant ink; acid-resistant ink can also be sprayed on the entire glass surface, which can omit the positioning operation required during spraying and avoid the problem of acid-resistant ink being sprayed on the preset matte area, causing poor gloss-matte effect, thereby simplifying the operation of spraying ink.

[0008] Preferably, before spraying the acid-resistant ink, the glass is clamped with a jig, and other areas of the glass except the preset smooth surface area are blocked by the jig, and then the acid-resistant ink is sprayed on the entire glass and the jig.

[0009] Preferably, before spraying the acid-resistant ink, the glass is clamped with a jig, and except for the preset smooth surface area and a portion of the shielding film near the preset smooth surface area, the other areas of the glass are shielded by the jig, and then the acid-resistant ink is sprayed on the entire glass and the jig.

[0010] Preferably, when the glass is clamped by the jig, the preset matte area of ​​the glass is completely covered by the masking film.

[0011] Preferably, when the glass is clamped by a jig, the preset matte area of ​​the glass is partially covered by a shielding film, and the shielding film is attached along the edge of the preset glossy area.

[0012] Use a jig to clamp the glass and cover the preset matte area of ​​the glass, and then spray the glass and the jig as a whole, so as to omit the positioning operation required for spraying, and avoid the problem of acid-resistant ink being sprayed into the preset matte area, causing poor matte effect, which can simplify the operation of spraying ink.

[0013] Except for the preset glossy area and a portion of the shielding film close to the preset glossy area, other areas of the glass are shielded by the jig, which can avoid the problem that the jig itself has a certain thickness, which will cause the edge of the preset glossy area close to the jig to not be completely sprayed with acid-resistant ink during spraying, and cannot play a protective role, thereby affecting the matte effect; exposing a portion of the shielding film close to the preset glossy area can avoid the problem that the preset glossy area cannot be completely sprayed with acid-resistant ink.

[0014] When using a jig to clamp the glass, the preset matte area of ​​the glass is partially covered by the masking film, and the masking film is attached along the edge of the preset glossy area. This can save the amount of masking film, and the smaller area of ​​masking film is easy to attach, which can avoid uneven attachment, resulting in the problem of masking film warping during the later surface drying and baking process.

[0015] If the other side of the glass does not need to be AG etched, acid-resistant ink can be sprayed on the other side of the glass for protection when spraying the ink.

[0016] Preferably, the shielding film is a high temperature resistant shielding film.

[0017] Preferably, the thickness of the shielding film is 40-60 μm.

[0018] Choosing a masking film of appropriate thickness can make the interface between glossy and matte surfaces neatly distinguishable and beautiful in appearance.

[0019] Preferably, the shielding film comprises: a film layer and an adhesive coated on the surface of the film layer, and the raw materials of the adhesive include, by weight: 55-65 parts of vinyl silicone oil, 35-45 parts of hydroxy vinyl MQ silicone resin, 0.8-1.2 parts of modified carbon fiber, 1-1.5 parts of catalyst, 1-2 parts of hydrogenated silicone oil and 100 parts of organic solvent.

[0020] Preferably, in the process of preparing the modified carbon fiber, the carbon fiber grafted with amino groups, epoxy POSS and isopropanol are mixed, kept warm at 60-80° C. for 1-2 hours, and the solid-liquid is separated to obtain the modified carbon fiber.

[0021] Preferably, in the process of preparing the modified carbon fiber, the carbon fiber grafted with amino groups is obtained by grafting and modifying the carbon fiber with a silane coupling agent containing amino groups.

[0022] Preferably, in the process of preparing the modified carbon fiber, the weight ratio of the carbon fiber grafted with amino groups, epoxy POSS and isopropanol is 1:3-5:100.

[0023] The amino-containing silane coupling agent may be 3-aminopropyltriethoxysilane, and the epoxy POSS may be epoxycyclohexyl-cage polysilsesquioxane.

[0024] Preferably, the catalyst is chloroplatinic acid-divinyltetramethyldisiloxane.

[0025] Preferably, the organic solvent is at least one of ethyl acetate, toluene and ethanol.

[0026] Preferably, the film layer is a polyimide film layer.

[0027] Preferably, the raw materials of the adhesive are mixed and degassed, and then coated on one side of the film layer, left to stand to volatilize the organic solvent, and then heated at 70-90° C. for 20-30 minutes to obtain a shielding film.

[0028] The present invention uses a polyimide film layer and an organosilicon adhesive, so that the shielding film has good high temperature resistance; and uses epoxy POSS to graft amino carbon fibers, and realizes grafting modification through the reaction of epoxy groups and amino groups, thereby improving the compatibility of carbon fibers in vinyl silicone oil and hydroxy vinyl MQ silicone resin, and the remaining epoxy groups on the modified carbon fibers can be further reacted and connected with the hydroxyl groups in the hydroxy vinyl MQ silicone resin, thereby introducing an appropriate amount of evenly distributed carbon fibers and POSS into the adhesive, thereby improving the adhesion performance of the shielding film to the glass and the problem of high-temperature residual glue; and an appropriate amount of vinyl silicone oil and hydrogen-containing silicone oil can increase the crosslinking density and mechanical strength of the adhesive, further improving the adhesion performance and the problem of residual glue; the present invention is aimed at the preparation process of the above-mentioned matte homologous glass, and specially develops the above-mentioned shielding film so that the shielding film does not have a warping phenomenon after surface drying and baking, and there is no residual glue phenomenon when the film is torn off, so that the matte junction can be neatly distinguished and the appearance is beautiful.

[0029] Using a jig to clamp the glass can further maintain the firmness of the masking film, and further avoid problems such as warping and falling off of the masking film when spraying acid-resistant ink, surface drying, and baking.

[0030] Preferably, the surface drying temperature is 80-100°C and the time is 5-10 minutes.

[0031] Preferably, the baking temperature is 160-180° C. and the baking time is 40-60 min.

[0032] Preferably, the glass is 2D glass, 2.5D glass or 3D glass.

[0033] Preferably, the polishing is chemical polishing.

[0034] Beneficial effects:

[0035] 1. The process of the present invention can replace the existing exposure and development technology. The cost of the present invention is about 60% lower than that of the exposure and development technology, and the process of the present invention can increase the production capacity by about 200%. The present invention is easy to operate and can be used for large-scale process production.

[0036] 2. Aiming at the preparation process of the matte homologous glass, the present invention has specially developed a shielding film with good high temperature resistance and strong adhesion; after surface drying and baking, the shielding film will not warp, and there will be no residual glue when the film is torn off, so that the interface between the matte and matte can be neatly distinguished, the appearance is beautiful, and it meets customer requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 Schematic diagram of the attachment position of the shielding film on the 3D glass in Examples 2 and 3.

[0038] Figure 2Schematic diagram of the positions of the fixture, shielding film and 3D glass in Example 3.

[0039] Figure 3 This is a photo of the matte homogeneous 3D glass prepared in Example 3. DETAILED DESCRIPTION

[0040] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.

[0041] Example 1

[0042] A process for preparing matt homogeneous glass comprises the following steps:

[0043] Take 3D glass, the convex surface of the glass includes a preset glossy area and a preset matte area, and attach a shielding film with a thickness of 40 μm to the glass, so that the preset glossy area is exposed and the preset matte area is completely covered by the shielding film;

[0044] Then, the convex surface of the 3D glass is placed upward on the carrier plate of the spraying machine assembly line, and enters the spraying machine to spray the acid-resistant ink on the preset glossy area (or the entire convex surface of the 3D glass). Then, the 3D glass follows the carrier plate into the tunnel furnace and is surface dried at 100°C for 5 minutes. Then, the 3D glass is placed in the turnover tray, put into the oven, and baked at 180°C for 40 minutes to fully dry the acid-resistant ink on the surface of the 3D glass.

[0045] Then take out the 3D glass and cool it to room temperature, tear off the masking film, put it on the cleaning rack, and put it into the cleaning machine for cleaning. Then the cleaned 3D glass will be sent to the AG etching process for strong acid etching. After the etching is completed, except for the preset glossy area protected by acid-resistant ink, the glass surface in other areas will become matte. Then the 3D glass will be de-inked and chemically polished to obtain matte homogeneous glass.

[0046] The shielding film includes: a polyimide film layer and an adhesive coated on the surface of the polyimide film layer, and the raw materials of the adhesive include, by weight: 55g of vinyl silicone oil, 45g of hydroxy vinyl MQ silicone resin, 0.8g of modified carbon fiber, 1.5g of chloroplatinic acid-divinyltetramethyldisiloxane, 1g of hydrogenated silicone oil and 100g of ethanol;

[0047] In the process of preparing the modified carbon fiber, 1 g of carbon fiber grafted with 3-aminopropyltriethoxysilane, 5 g of epoxycyclohexyl-cage polysilsesquioxane and 100 g of isopropanol were mixed, kept warm at 60°C for 2 h, filtered, the filter cake was washed, and dried to obtain the modified carbon fiber;

[0048] The raw materials of the adhesive are mixed and degassed, and then coated on one side of the polyimide film layer. After standing to evaporate the ethanol, the film is heated at 70° C. for 30 minutes to obtain a masking film.

[0049] Example 2

[0050] A process for preparing matt homogeneous glass comprises the following steps:

[0051] Take 3D glass, the convex surface of the glass includes a preset glossy area and a preset matte area, and attach a shielding film with a thickness of 60 μm along the edge of the preset glossy area, so that the preset glossy area is exposed and the preset matte area is partially covered (such as Figure 1 As shown, the portion of the shielding film that exceeds the 3D glass can be folded back to the concave surface of the 3D glass);

[0052] Then, the 3D glass is clamped with a jig so that, except for the preset glossy area, other areas of the glass are blocked by the jig. Then, the jig with the 3D glass is placed on the carrier plate of the spraying machine assembly line so that the convex surface of the 3D glass faces upward and enters the spraying machine. The 3D glass and the jig are sprayed with acid-resistant ink as a whole. Then, the 3D glass and the jig follow the carrier plate into the tunnel furnace and are dried at 80°C for 10 minutes. Then, the 3D glass and the jig are placed in a turnover tray, put into an oven, and baked at 160°C for 60 minutes to fully dry the acid-resistant ink on the surface of the 3D glass.

[0053] Then take out the 3D glass and cool it to room temperature, tear off the masking film, put it on the cleaning rack, and put it into the cleaning machine for cleaning. Then the cleaned 3D glass will be sent to the AG etching process for strong acid etching. After the etching is completed, except for the preset glossy area protected by acid-resistant ink, the glass surface in other areas will become matte. Then the 3D glass will be de-inked and chemically polished to obtain matte homogeneous glass.

[0054] The shielding film includes: a polyimide film layer and an adhesive coated on the surface of the polyimide film layer, and the raw materials of the adhesive include, by weight: 65g of vinyl silicone oil, 35g of hydroxy vinyl MQ silicone resin, 1.2g of modified carbon fiber, 1g of chloroplatinic acid-divinyltetramethyldisiloxane, 2g of hydrogenated silicone oil and 100g of ethanol;

[0055] In the process of preparing the modified carbon fiber, 1 g of carbon fiber grafted with 3-aminopropyltriethoxysilane, 3 g of epoxycyclohexyl-cage polysilsesquioxane and 100 g of isopropanol were mixed, kept warm at 80°C for 1 hour, filtered, the filter cake was washed, and dried to obtain the modified carbon fiber;

[0056] The raw materials of the adhesive are mixed and degassed, and then coated on one side of the polyimide film layer. After standing to evaporate the ethanol, the film is heated at 90° C. for 20 minutes to obtain a masking film.

[0057] Example 3

[0058] A process for preparing matt homogeneous glass comprises the following steps:

[0059] Take 3D glass, the convex surface of the glass includes a preset glossy area and a preset matte area, and attach a shielding film with a thickness of 50 μm along the edge of the preset glossy area, so that the preset glossy area is exposed and the preset matte area is partially covered (such as Figure 1 As shown, the portion of the shielding film that exceeds the 3D glass can be folded back to the concave surface of the 3D glass);

[0060] Then, the 3D glass is clamped with a fixture so that, except for the preset glossy area and a portion of the shielding film near the preset glossy area, the other areas of the glass are blocked by the fixture (such as Figure 2 As shown), the jig with the 3D glass is then placed on the carrier plate of the spraying machine assembly line, so that the convex surface of the 3D glass faces upward, and enters the spraying machine, and the acid-resistant ink is sprayed on the 3D glass and the jig as a whole. Then, the 3D glass and the jig follow the carrier plate into the tunnel furnace, and the surface is dried at 100°C for 8 minutes; then, the 3D glass and the jig are placed in a turnover tray, put into an oven, and baked at 180°C for 40 minutes to fully dry the acid-resistant ink on the surface of the 3D glass;

[0061] Then take out the 3D glass and cool it to room temperature, tear off the masking film, put it on the cleaning rack, and put it into the cleaning machine for cleaning. Then the cleaned 3D glass will be sent to the AG etching process for strong acid etching. After the etching is completed, except for the preset glossy area protected by acid-resistant ink, the glass surface in other areas will become matte. Then the 3D glass will be de-inked and chemically polished to obtain matte homogeneous glass.

[0062] The shielding film includes: a polyimide film layer and an adhesive coated on the surface of the polyimide film layer, and the raw materials of the adhesive include, by weight: 60 g of vinyl silicone oil, 40 g of hydroxy vinyl MQ silicone resin, 1 g of modified carbon fiber, 1.2 g of chloroplatinic acid-divinyltetramethyldisiloxane, 1.5 g of hydrogenated silicone oil and 100 g of ethanol;

[0063] In the process of preparing the modified carbon fiber, 1 g of carbon fiber grafted with 3-aminopropyltriethoxysilane, 4 g of epoxycyclohexyl-cage polysilsesquioxane and 100 g of isopropanol were mixed, kept warm at 70°C for 1.5 h, filtered, the filter cake was washed, and dried to obtain the modified carbon fiber;

[0064] The raw materials of the adhesive are mixed and degassed, and then coated on one side of the polyimide film layer. After standing to evaporate the ethanol, the film is heated at 80° C. for 25 minutes to obtain a masking film.

[0065] Comparative Example 1

[0066] The matte homogeneous 3D glass is manufactured by using exposure and development technology. The specific steps of the exposure and development technology are as follows: take 3D glass, spray exposure and development acid-resistant ink on the entire convex surface of the 3D glass, then locally expose and UV cure the preset glossy area, then use KOH aqueous solution to clean the oil film that has not been UV cured in other areas, and then sequentially perform baking, cleaning, strong acid etching, ink removal, and chemical polishing to obtain matte homogeneous glass; wherein, the size, material, and preset glossy area of ​​the 3D glass are the same as those in Example 3, and the baking, cleaning, strong acid etching, ink removal, and chemical polishing processes are the same as those in Example 3.

[0067] 1000 sheets of matte homogeneous 3D glass were prepared respectively by the methods of Examples 1-3 and Comparative Example 1, and the total time consumption and product yield were counted. The results are shown in Table 1.

[0068] Table 1 Statistical results

[0069]

[0070]

[0071] It can be seen from Table 1 that the production cycle of Examples 1-3 is shorter than that of Comparative Example 1, the yield rate of the obtained matte homogeneous 3D glass is higher than that of Comparative Example 1, and the phenomenon of warping and residual adhesive rarely occurs.

[0072] Typical matte 3D glass photos Figure 3 As shown, Figure 3 This is a photo of the matte homogeneous 3D glass prepared in Example 3.

[0073] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A process for preparing matt homogeneous glass, characterized in that: The method comprises the following steps: taking glass, one side of the glass comprises a preset glossy area and a preset matte area, attaching a shielding film on the glass so that the preset glossy area is exposed, spraying acid-resistant ink on the preset glossy area, and then sequentially performing surface drying, baking, film tearing, cleaning, AG etching, ink removal, and polishing to obtain glossy and matte homogeneous glass; The masking film comprises: a film layer and an adhesive coated on the surface of the film layer, wherein the raw materials of the adhesive comprise, by weight, 55-65 parts of vinyl silicone oil, 35-45 parts of hydroxy vinyl MQ silicone resin, 0.8-1.2 parts of modified carbon fiber, 1-1.5 parts of catalyst, 1-2 parts of hydrogenated silicone oil and 100 parts of organic solvent; In the process of preparing the modified carbon fiber, carbon fiber grafted with amino groups, epoxy POSS and isopropanol are mixed, kept warm at 60-80° C. for 1-2 hours, and solid-liquid separation is performed to obtain the modified carbon fiber; In the process of preparing modified carbon fiber, carbon fiber grafted with amino group is obtained by grafting and modifying carbon fiber with silane coupling agent containing amino group; In the preparation process of the modified carbon fiber, the weight ratio of the carbon fiber grafted with amino groups, epoxy POSS and isopropanol is 1:3-5:100; The film layer is a polyimide film layer.

2. The process for preparing matt homogeneous glass according to claim 1, characterized in that: The intended matte areas of the glass are completely covered with masking film.

3. The process for preparing matt homogeneous glass according to claim 1, characterized in that: Before spraying the acid-resistant ink, the glass is clamped with a jig. Except for the preset glossy area, other areas of the glass are blocked by the jig. Then, the acid-resistant ink is sprayed on the entire glass and the jig.

4. The process for preparing matt homogeneous glass according to claim 1, characterized in that: Before spraying the acid-resistant ink, the glass is clamped with a jig, and the other areas of the glass are blocked by the jig except for the preset glossy area and a part of the shielding film close to the preset glossy area, and then the acid-resistant ink is sprayed on the entire glass and the jig.

5. The process for preparing matt homogeneous glass according to claim 3 or 4, characterized in that: When the glass is clamped with a jig, the preset matte area of ​​the glass is completely covered by the masking film.

6. The process for preparing matt homogeneous glass according to claim 3 or 4, characterized in that: When the glass is clamped by the jig, the preset matte area of ​​the glass is partially covered by the masking film, and the masking film is attached along the edge of the preset glossy area.

7. The process for preparing matt homogeneous glass according to claim 1, characterized in that: The shielding film is a high temperature resistant shielding film.

8. The process for preparing matt homogeneous glass according to claim 1, characterized in that: The thickness of the masking film is 40-60 μm.

9. The process for preparing matt homogeneous glass according to claim 1, characterized in that: Catalyst: chloroplatinic acid-divinyltetramethyldisiloxane.

10. The process for preparing matt homogeneous glass according to claim 1, characterized in that: The organic solvent is at least one of ethyl acetate, toluene and ethanol.

11. The process for preparing matt homogeneous glass according to claim 1, characterized in that: The raw materials of the adhesive are mixed and degassed, and then coated on one side of the film layer, left to stand to volatilize the organic solvent, and then heated at 70-90° C. for 20-30 minutes to obtain a masking film.

12. The process for preparing matt homogeneous glass according to claim 1, characterized in that: The surface drying temperature is 80-100°C and the time is 5-10 minutes.

13. The process for preparing matt homogeneous glass according to claim 1, characterized in that: The baking temperature is 160-180°C and the baking time is 40-60 minutes.

14. The process for preparing matt homogeneous glass according to claim 1, characterized in that: The glass includes 2D glass, 2.5D glass and 3D glass.

15. The process for preparing matt homogeneous glass according to claim 1, characterized in that: Polishing is chemical polishing.

Citation Information

Patent Citations

  • Glass processing method

    CN105693101A

  • Manufacturing method of anti-glare glass shell, anti-glare glass shell and electronic equipment

    CN111943519A

  • Glass cover plate with different AG combination effects and preparation method thereof

    CN113391381A

  • Protection method before local AG of TP glass

    CN113562982A

  • Local AG (anti-glare) glass and preparation method thereof

    CN114426401A