A flue gas denitration catalyst and preparation method thereof
In the preparation of flue gas denitrogenation catalyst, the activity and molding of catalysts under high airspeed conditions are solved by using the lattice defects of titanium and aluminum and the complement of tungsten, and combined with the use of polymer dispersants and pore-forming agents. An efficient formation process of flue gas denitrification and cost-reducing formation is achieved.
Patent Information
- Application Number
- CN202111681121.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-31
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-12-31
AI Technical Summary
The existing flue gas denitrification catalysts are unevenly dispersed under high airspeed conditions, resulting in low denitrification efficiency and unstable catalytic activity. They are prone to cracks or bonds during the molding process, resulting in low molding rate and insufficient mechanical strength, which increases cost.
After mixing the titanium source precursor and aluminum source precursor solution, the pH precursor is adjusted, and then evenly mixed with the tungsten source precursor, binder, pore-forming agent and polymer dispersant, it is stamped and modularly assembled, combined with The resin glue is then stacked and assembled, and finally roasted at high temperature to stabilize the catalyst structure.
It improves the dispersion uniformity of the active components of the catalyst and the stability of catalytic activity, increases the external specific surface area, reduces the molding cost, increases the molding rate and mechanical strength, and is suitable for flue gas denitrition under high aerial speed conditions.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalysts, and in particular relates to a flue gas denitration catalyst and a preparation method thereof. Background Art
[0002] Nitrogen oxides (NO x ) is one of the main air pollutants, and emission requirements are becoming increasingly stringent. Among the many flue gas denitrification technologies, the selective catalytic reduction method SCR is still the international mainstream technology, and its NOx removal rate can reach 80% to 90%. Among them, the denitrification catalyst is the core of SCR technology. Developed countries developed a series of denitrification catalysts for different boiler types in the 1980s. According to the different molding methods, they are divided into corrugated plate type, honeycomb type and plate type to meet the requirements of different flue gas working conditions.
[0003] CN111330634A proposes a method for a corrugated plate denitration catalyst, wherein graphene, nano-titanium dioxide, porous molecular sieve, molybdenum trioxide, tungsten trioxide, ammonium metavanadate, oxalic acid and water are mixed to obtain a mixed solution, ammonia water is used to adjust the pH value of the mixed solution to 6-7, and then the mixture is stirred, mixed, left to stand and dehydrated to obtain a denitration catalyst slurry; the slurry is solidified and mixed with ethylene-vinyl acetate copolymer and glass fiber to obtain a denitration catalyst mud material, the denitration catalyst mud material is stamped and formed to obtain a corrugated sheet, a resin glue is sprayed between several sheets of the corrugated sheets and then stacked and assembled to obtain a corrugated plate denitration catalyst blank, and the corrugated plate denitration catalyst blank is fired to obtain a corrugated plate denitration catalyst. The catalyst prepared by this method contains active ingredients in the corrugated plate structure substrate and has a large specific surface area, but the raw materials used fail to achieve atomic-level mixing, resulting in insufficient catalyst active sites, and may also cause a high degree of aggregation of the same material, which will have a certain impact on the catalyst activity.
[0004] CN103143396B proposes a method for preparing a corrugated plate denitration catalyst, wherein titanium dioxide, silicon dioxide, and an active substance are mixed into a slurry, and then a binder, glass fiber, etc. are added, and finally extrusion molding is performed. The method is simple in process, but the active substance is not well dispersed, resulting in a low denitration efficiency of the catalyst.
[0005] CN 107138150 B discloses a honeycomb denitration catalyst, which is prepared from the following components in parts by weight: 70-90 parts of titanium dioxide, 2-16 parts of tungsten trioxide, 1.0-3 parts of vanadium pentoxide, and 0.5-3 parts of pore-forming agent. The denitration catalyst of the invention has the advantages of high catalytic efficiency, small amount of catalyst and low cost. CN 107096524 B discloses a honeycomb low-temperature denitration catalyst and a preparation method thereof, which uses a honeycomb denitration catalyst including titanium dioxide, tungsten trioxide, ammonium metavanadate and the like as components and a preparation method thereof, resists heavy metal and sulfide poisoning, and prolongs service life, but these catalysts are currently generally suitable for preparing honeycomb catalysts with no more than 50 holes to meet denitration sites with lower air velocity requirements. In order to meet the actual needs of denitrification with higher space velocity requirements, the catalyst needs to be processed into a honeycomb catalyst with more pores to increase its external specific surface area. The porous honeycomb catalyst is prone to cracks or stick to the mold during extrusion, and has a low molding rate and low mechanical strength, resulting in a waste of production resources and increased costs.
[0006] Therefore, those skilled in the art still need to conduct further research on the corrugated plate flue gas denitrification catalyst with high space velocity requirements. Summary of the invention
[0007] The main purpose of the present invention is to provide a flue gas denitration catalyst and a preparation method thereof, so as to overcome the defects of the prior art denitration catalyst such as uneven dispersion of active components, low denitration efficiency of the catalyst, unstable catalytic activity, etc.
[0008] In order to achieve the above object, the present invention provides a method for preparing a flue gas denitration catalyst, comprising the following steps:
[0009] Step 1, mixing a titanium source precursor solution and an aluminum source precursor solution, adjusting the pH value to 7-12, and precipitating;
[0010] Step 2, mixing the precipitate obtained in step 1 with an alkali solution, stirring, and obtaining a secondary precipitate;
[0011] Step 3, mixing the secondary precipitate with a tungsten source precursor solution, drying, and calcining to obtain an intermediate powder;
[0012] Step 4, mixing the intermediate powder with the vanadium source precursor solution, the polymer dispersant, the binder, and the pore-forming agent, adjusting the pH value to 7 to 12, and uniformly mixing to form a slurry;
[0013] Step 5, stamping the slurry obtained in step 4 to obtain corrugated sheets, spraying resin glue between the corrugated sheets and stacking and assembling them to obtain corrugated plate type denitration catalyst blanks, drying and roasting them to obtain corrugated plate type flue gas denitration catalysts.
[0014] The preparation method of the flue gas denitration catalyst of the present invention, wherein in the step 5, the calcination is programmed to heat according to the following process: the dried corrugated plate denitration catalyst blank is heated to a predetermined temperature of 450-680°C, the heating rate is controlled to be no more than 1°C / min, after the temperature reaches the predetermined temperature, it is calcined at a constant temperature for 2-40 hours, and then cooled at a cooling rate of no more than 4°C / min to below 50°C to obtain a corrugated plate flue gas denitration catalyst.
[0015] The preparation method of the flue gas denitration catalyst of the present invention, wherein, in step 1, the reagent for adjusting the pH value is ammonia water, and the pH value is adjusted to 7-12; the mixing method in step 4 is stirring or ultrasonic oscillation, and the mixing time is 0.1-8h; the water mass content of the slurry in step 4 is 5-40%.
[0016] The preparation method of the flue gas denitration catalyst of the present invention, wherein the polymer dispersant is at least one of polyethylene glycol, polyacrylamide, and polyvinyl pyrrolidone; the binder is at least one of carboxymethyl cellulose and hydroxypropyl cellulose; the pore-forming agent is at least one of polyethylene oxide, polymethyl methacrylate, and sesbania powder; the titanium source precursor solution is TiO 2 The mass ratio of the polymer dispersant to the titanium source precursor solution is 0.1 to 2.0:100, the mass ratio of the binder to the titanium source precursor solution is 0.1 to 2.0:100, and the mass ratio of the pore former to the titanium source precursor solution is 0.1 to 2.0:100.
[0017] The preparation method of the flue gas denitration catalyst of the present invention, wherein the calcination temperature in step 3 and step 5 is 450-680°C, and the calcination time is 2-40h; glass fiber is also added in step 4, and the titanium source precursor solution is TiO 2 The mass ratio of the glass fiber to the titanium source precursor solution is 2 to 10:100.
[0018] The corrugated plate catalyst obtained in step 5 has a corrugated plate thickness of 0.2 to 0.6 mm, a corrugated width of 4 to 8 mm, and a corrugated height of 4 to 10 mm.
[0019] In order to achieve the above object, the present invention also provides a flue gas denitration catalyst obtained by the above preparation method.
[0020] Beneficial effects of the present invention:
[0021] The present invention utilizes a strong alkali to dissolve aluminum atoms in a titanium-aluminum lattice, thereby greatly increasing the lattice defects of the titanium substrate. The lattice defects of aluminum dissolved by the strong alkali are at the surface position that is easy to contact with flue gas in a flue gas atmosphere. After being supplemented by the catalytic promoter component, the SCR catalytic activity can be more effectively exerted, thereby improving the denitration effect under the same conditions. Tungsten element is added to the titanium substrate after the aluminum element is dissolved. Since there are more lattice defects, the tungsten element is supplemented, and the lattice defects of the hybrid substrate are more stable after calcination. At the same time, the crystal form of the titanium substrate can remain in the anatase type without crystallization during high-temperature calcination, which is more conducive to the catalyst maintaining a high denitration activity.
[0022] The present invention adopts pore-forming agent, binder, glass fiber and other additives to prepare the catalyst into a corrugated plate catalyst with good activity and strength, which is conducive to its modular assembly and long-term stable operation on an industrial denitration device.
[0023] DeNOx catalysts with large external specific surface areas have certain technical difficulties in preparation. The catalysts are prone to cracks or stick to the mold during extrusion, and have low molding rates and mechanical strength, resulting in high production costs and high transportation damage rates. Corrugated plate catalysts have larger external specific surface areas, high molding rates, low production costs, and are easy to transport and have low damage rates. They reduce catalyst loading space and reduce device investment costs. Corrugated plate deNOx catalysts have overcome this problem better. DETAILED DESCRIPTION
[0024] The following is a detailed description of the embodiments of the present invention. The embodiments are implemented based on the technical solution of the present invention, and detailed implementation methods and processes are given. However, the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments where specific conditions are not specified are usually based on conventional conditions.
[0025] The present invention provides a method for preparing a flue gas denitration catalyst, comprising the following steps:
[0026] Step 1, mixing a titanium source precursor solution and an aluminum source precursor solution, adjusting the pH value to 7-12, and precipitating;
[0027] Step 2, mixing the precipitate obtained in step 1 with an alkali solution, stirring, and obtaining a secondary precipitate;
[0028] Step 3, mixing the secondary precipitate with a tungsten source precursor solution, drying, and calcining to obtain an intermediate powder;
[0029] Step 4, mixing the intermediate powder with the vanadium source precursor solution, the polymer dispersant, the binder, and the pore-forming agent, adjusting the pH value to 7 to 12, and uniformly mixing to form a slurry;
[0030] Step 5, stamping the slurry obtained in step 4 to obtain corrugated sheets, spraying resin glue between the corrugated sheets and stacking and assembling them to obtain corrugated plate type denitration catalyst blanks, drying and roasting them to obtain corrugated plate type flue gas denitration catalysts.
[0031] In one embodiment, the titanium source precursor is a soluble titanium-containing compound, such as a titanium-containing compound soluble in water. In another embodiment, the titanium source precursor is at least one of titanyl sulfate and metatitanic acid, and the titanium source precursor solution is a solution formed by the titanium source precursor. Further, the titanium source precursor solution is a solution formed by dissolving the titanium source precursor in water, and the solution contains an acid solution, such as sulfuric acid, nitric acid, etc. In another embodiment, the titanium source precursor solution is TiO 2 The calculated concentration is 15-35 g / L.
[0032] In one embodiment, the aluminum source precursor is a soluble aluminum-containing compound, such as an aluminum-containing compound soluble in water. In another embodiment, the aluminum source precursor is aluminum sulfate or aluminum nitrate, and the aluminum source precursor solution is a solution formed by the aluminum source precursor, and further, the aluminum source precursor solution is a solution formed by dissolving the aluminum source precursor in water.
[0033] In one embodiment, the titanium source precursor solution is TiO 2 The aluminum source precursor solution is based on Al 2 O 3 The mass ratio of the titanium source precursor solution to the aluminum source precursor solution is 100:0.3-5.0.
[0034] After the titanium source precursor solution and the aluminum source precursor solution are mixed, the pH value of the mixed solution is adjusted to 7 to 12, and then precipitated, washed, and filtered. In one embodiment, the pH value of the mixed solution is adjusted to 7.5 to 10. The present invention does not particularly limit the reagent used to adjust the pH value, for example, it can be ammonia water.
[0035] The present invention utilizes an in-situ mixing method to mix titanium atoms and aluminum atoms at the molecular level, so that crystals with lattice defects are generated in the subsequent titanium-aluminum co-precipitation process, and the particle size of the metal oxide in the precipitate is small and uniform.
[0036] Step 2 is to mix the precipitate obtained in step 1 with an alkali solution, and stir to obtain a secondary precipitate.
[0037] In one embodiment, the alkali solution is a strong alkali solution; in another embodiment, the alkali solution is an alkali metal hydroxide solution or an alkaline earth metal hydroxide solution, such as a sodium hydroxide solution, a potassium hydroxide solution, etc. In another embodiment, the concentration of the alkali solution is 0.5 to 5 mol / L, and the amount of the alkali solution used is 1 to 5 times the mass of the precipitate obtained in step 1.
[0038] The present invention utilizes a strong base to dissolve the aluminum atoms in the titanium-aluminum lattice, which greatly increases the lattice defects of the titanium substrate. The lattice defects of the aluminum dissolved by the strong base are easily exposed to the surface position of the flue gas in the flue gas atmosphere. After being supplemented by the co-catalytic components, the SCR catalytic activity can be more effectively exerted, thereby enhancing the denitrification effect under the same conditions.
[0039] Step 3 is to mix the secondary precipitate with the tungsten source precursor solution, dry, roast and grind to obtain an intermediate powder.
[0040] In one embodiment, the tungsten source precursor is a soluble tungsten-containing compound, such as a tungsten-containing compound soluble in water. In another embodiment, the tungsten source precursor is at least one of an ammonium paratungstate solution and an ammonium metatungstate solution, and the tungsten source precursor solution is a solution formed by the tungsten source precursor, and further, the tungsten source precursor solution is a solution formed by the tungsten source precursor dissolved in water. In another embodiment, the tungsten source precursor solution is calculated as tungsten trioxide, and the titanium source precursor solution is calculated as TiO 2 The mass ratio of the tungsten source precursor solution to the titanium source precursor solution is 0.5-6.0:100.
[0041] In one embodiment, the calcination temperature in step 3 is preferably 450-680° C., and the calcination time is preferably 2-40 hours.
[0042] The present invention supplements tungsten element on the titanium substrate after the aluminum element is dissolved. Since there are more lattice defects, the tungsten element fills the position. After roasting, the lattice defects of the hybrid substrate are more stable. At the same time, the crystal form of the titanium substrate can remain in the anatase type without crystal transformation during high-temperature roasting, which is more conducive to the catalyst maintaining a high denitrification effect.
[0043] Step 4 is to mix the intermediate powder with the vanadium source precursor solution, the polymer dispersant, the binder, and the pore-forming agent, adjust the pH value to 7 to 12, and evenly mix them to form a slurry.
[0044] In one embodiment, the vanadium source precursor is a soluble vanadium-containing compound, such as a vanadium-containing compound soluble in water. In another embodiment, the vanadium source precursor is at least one of an ammonium metavanadate solution and an ammonium vanadate solution, and the vanadium source precursor solution is a solution formed by the vanadium source precursor, and further, the vanadium source precursor solution is a solution formed by the vanadium source precursor dissolved in water. In another embodiment, the vanadium source precursor solution is V 2 O 5 The titanium source precursor solution is based on TiO 2 The mass ratio of the vanadium source precursor solution to the titanium source precursor solution is 0.2-5.0:100.
[0045] Under the action of the polymer dispersant, the vanadium source of the catalyst of the present invention can be fully dispersed on the hybridized substrate. At the same time, due to the influence of the co-catalyst component tungsten on the substrate with larger lattice defects, vanadium penetrates deeper into the surface of the titanium-tungsten particles, connects more tightly, and disperses more evenly. After calcination, the catalyst activity is higher and more stable.
[0046] In one embodiment, the polymer dispersant is at least one of polyethylene glycol, polyacrylamide, and polyvinyl pyrrolidone. 2 The mass ratio of the polymer dispersant to the titanium source precursor solution is 0.1 to 2.0:100.
[0047] In one embodiment, the binder is at least one of carboxymethyl cellulose and hydroxypropyl cellulose; the pore-forming agent is at least one of polyethylene oxide, polymethyl methacrylate, and sesbania powder; the titanium source precursor solution is TiO 2 The mass ratio of the binder to the titanium source precursor solution is 0.1 to 2.0:100, and the mass ratio of the pore former to the titanium source precursor solution is 0.1 to 2.0:100.
[0048] In another embodiment, glass fiber is further added in step 4, and the titanium source precursor solution is TiO 2 The mass ratio of glass fiber to titanium source precursor solution is 2 to 10:100.
[0049] In another embodiment, the water content of the slurry in step 4 is 5-40%. In another embodiment, the mixing method in step 4 is stirring or ultrasonic oscillation, and the mixing time is 0.1-8 hours.
[0050] Step 5: stamping the slurry obtained in step 4 to obtain corrugated sheets, spraying resin glue between the corrugated sheets and stacking and assembling them to obtain corrugated plate type denitration catalyst blanks, drying and calcining them to obtain corrugated plate type flue gas denitration catalysts.
[0051] The present invention adopts pore-forming agent, binder, glass fiber and other additives to prepare the catalyst into a corrugated plate catalyst with good activity and strength, which is conducive to its modular assembly and long-term stable operation on an industrial denitration device.
[0052] In one embodiment, the calcination temperature in step 5 is 450-680°C, and the calcination time is 2-40 hours. The resin glue is, for example, epoxy resin glue. In the step 5, the calcination is programmed to heat up according to the following process: the dried corrugated plate type denitration catalyst blank is heated to a predetermined temperature of 450-680°C, and the heating rate is controlled to be no more than 1°C / min. After the temperature reaches the predetermined temperature, it is calcined at a constant temperature for 2-40 hours, and then cooled down at a cooling rate of no more than 4°C / min to below 50°C to obtain a corrugated plate type flue gas denitration catalyst.
[0053] In one embodiment, the corrugated plate catalyst obtained in step 5 preferably has a corrugated plate thickness of 0.2 to 0.6 mm, a corrugated width of 4 to 8 mm, and a corrugated height of 4 to 10 mm.
[0054] Therefore, the present invention provides a method for preparing a flue gas denitration catalyst. The active components of the corrugated plate flue gas denitration catalyst obtained by the method are evenly dispersed, the catalyst has high catalytic denitration activity, and the catalyst has stable catalytic activity.
[0055] The technical solution of the present invention will be further described below through specific embodiments.
[0056] Evaluation method:
[0057] NOx conversion rate evaluation conditions: air velocity 13000h -1 , reaction temperature 370℃, intake NOx 600mg / Nm 3 、SO 2 800mg / Nm 3 , the ammonia nitrogen ratio is 1.
[0058] NOx、SO 2 Concentration determination method: Flue gas continuous online analyzer, Siemens ULTRAMAT23.
[0059] SO 2 / SO 3 Conversion rate determination method: Limestone-gypsum wet flue gas desulfurization unit performance acceptance test specification (DL / T998-2006).
[0060] Embodiment 1:
[0061] Containing TiO 2 100 g of titanium sulfate was dissolved in sulfuric acid to form a solution; 2 O 3 1g of aluminum sulfate was dissolved in deionized water to form a solution. After the above two solutions were evenly mixed, the pH value was adjusted to 10 with ammonia water, precipitated, filtered, and washed; the washed material was placed in a 1mol / L sodium hydroxide solution of 3 times the mass of the powder, stirred for 8 hours, fully washed and filtered; the filtered material was made into a slurry with a water content of 45% with deionized water, and WO was added 3 2g of ammonium metatungstate solution was stirred for 3h and then dried, calcined at 550℃ for 2h, and ground into powder; the powder was then mixed with V 2 O 51g of ammonium metavanadate solution and 0.8g of polyvinyl pyrrolidone are evenly mixed, and then 0.6g of polyethylene oxide, 3g of glass fiber, 6g of carboxymethyl cellulose and deionized water are added and evenly mixed to form a mud material containing 25% water. The pH value is adjusted to 8.3, and corrugated plates are punched out. Epoxy resin glue is sprayed between the corrugated plates and then stacked and assembled to obtain a corrugated plate type denitration catalyst blank. After the embryo is dried, it is calcined at 600°C for 9h according to a heating program to obtain a corrugated plate type denitration catalyst.
[0062] The catalyst NO x Conversion rate 97.2%, SO 2 / SO 3 Conversion rate 0.67.
[0063] Example 2
[0064] Containing TiO 2 100 g of titanium sulfate was dissolved in sulfuric acid to form a solution; 2 O 3 3g of aluminum nitrate was dissolved in deionized water to form a solution. After the above two solutions were evenly mixed, the pH value was adjusted to 9.5 with ammonia water, precipitated, filtered and washed; the washed material was placed in a 2mol / L sodium hydroxide solution of 1 times the mass of the powder, stirred for 1h, fully washed and filtered; the filtered material was made into a slurry with a water content of 32% with deionized water, and WO was added 3 3g of ammonium paratungstate solution was stirred for 3h and then dried, calcined at 550℃ for 4h, and ground into powder; the powder was then mixed with V 2 O 5 1.5g of ammonium metavanadate solution and 1.0g of polyvinyl pyrrolidone were evenly mixed, and then 1g of polyethylene oxide, 3g of glass fiber, 5g of carboxymethyl cellulose and deionized water were added and evenly mixed to form a mud material containing 34% water. The pH value was adjusted to 8.5, and corrugated plates were punched out. Epoxy resin glue was sprayed between the corrugated plates and then stacked and assembled to obtain a corrugated plate type denitration catalyst blank. After the blank was dried, it was calcined at 620°C for 15h according to a heating program to obtain a corrugated plate type denitration catalyst.
[0065] The catalyst NO x Conversion rate 99.0%, SO 2 / SO 3 Conversion rate 0.77.
[0066] Example 3
[0067] Containing TiO 2 100 g of titanium sulfate was dissolved in sulfuric acid to form a solution; 2 O 32g of aluminum sulfate was dissolved in deionized water to form a solution. After the above two solutions were evenly mixed, the pH value was adjusted to 9.5 with ammonia water, precipitated, filtered and washed; the washed material was placed in a 2mol / L sodium hydroxide solution with a mass of 3 times the powder, stirred for 9 hours, fully washed and filtered; the filtered material was made into a slurry with a water content of 50% with deionized water, and WO was added 3 6g of ammonium paratungstate solution was stirred for 5h and then dried, calcined at 580℃ for 4h, and ground into powder; the powder was then mixed with V 2 O 5 5g of ammonium vanadate solution and 6g of polyacrylamide are evenly mixed, and then 2g of polyethylene oxide, 2g of glass fiber, 8g of carboxymethyl cellulose and deionized water are added and evenly mixed to form a mud material with a water content of 27.5%. The pH value is adjusted to 9, and corrugated plates are punched out. Epoxy resin glue is sprayed between the corrugated plates and then stacked and assembled to obtain a corrugated plate type denitration catalyst blank. After the blank is dried, it is calcined at 500°C for 9 hours according to a heating program to obtain a corrugated plate type denitration catalyst.
[0068] The fresh catalyst obtained above was evaluated. Evaluation results: The fresh catalyst NO x Conversion rate 97.8%, SO 2 / SO 3 Conversion rate 0.81.
[0069] Example 4
[0070] Containing TiO 2 100 g of titanium sulfate was dissolved in sulfuric acid to form a solution; 2 O 3 5g of aluminum nitrate was dissolved in deionized water to form a solution. After the above two solutions were evenly mixed, the pH value was adjusted to 10 with ammonia water, precipitated, filtered, and washed; the washed material was placed in a 2mol / L sodium hydroxide solution with a concentration of 2 times the mass of the powder, stirred for 9 hours, fully washed and filtered; the filtered material was made into a slurry with a water content of 40% with deionized water, and MO was added 3 2g of ammonium paratungstate solution was stirred for 5h and then dried, calcined at 500℃ for 4h, and ground into powder; the powder was then mixed with V 2 O 5 1.5g of ammonium metavanadate solution and 1g of polyacrylamide were evenly mixed, and then 1g of polyethylene oxide, 2g of glass fiber, 6g of hydroxypropyl cellulose and deionized water were added and evenly mixed to form a mud material containing 30% water. The pH value was adjusted to 8, and corrugated plates were punched out. Epoxy resin glue was sprayed between the corrugated plates and then stacked and assembled to obtain a corrugated plate type denitration catalyst blank. After the embryo was dried, it was calcined at 680°C for 4h according to a heating program to obtain a corrugated plate type denitration catalyst.
[0071] The fresh catalyst obtained above was evaluated. Evaluation results: the fresh catalyst NOx conversion rate was 98.8%, SO 2 / SO 3 Conversion rate 0.79.
[0072] Example 5
[0073] Containing TiO 2 100 g of titanium sulfate was dissolved in sulfuric acid to form a solution; 2 O 3 4g of aluminum nitrate was dissolved in deionized water to form a solution. After the above two solutions were evenly mixed, the pH value was adjusted to 9 with ammonia water, precipitated, filtered and washed; the washed material was placed in a 2mol / L sodium hydroxide solution with a mass of 5 times the powder, stirred for 2h, fully washed and filtered; the filtered material was made into a slurry with a water content of 30% with deionized water, and MO was added 3 0.5g of ammonium paratungstate solution was stirred for 3h and then dried, calcined at 450℃ for 3h, and ground into powder; the powder was then mixed with V 2 O 5 1g of ammonium metavanadate solution and 1g of polyacrylamide are evenly mixed, and then 1g of polyethylene oxide, 0.2g of sesbania powder, 2g of glass fiber, 10g of hydroxypropyl cellulose and deionized water are added and evenly mixed to form a mud material containing 35% water. The pH value is adjusted to 8.5, and corrugated plates are punched out. Epoxy resin glue is sprayed between the corrugated plates and then stacked and assembled to obtain a corrugated plate type denitrification catalyst blank. After the embryo is dried, it is calcined at 600°C for 4h according to a heating program to obtain a corrugated plate type denitrification catalyst.
[0074] The fresh catalyst obtained above was evaluated. Evaluation results: the fresh catalyst NOx conversion rate was 98.2%, SO 2 / SO 3 Conversion rate 0.64.
[0075] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a flue gas denitration catalyst, characterized in that: The steps include: Step 1, mixing a titanium source precursor solution and an aluminum source precursor solution, adjusting the pH value to 7-12, and precipitating; Step 2, mixing the precipitate obtained in step 1 with a strong alkaline solution, stirring, and obtaining a secondary precipitate; Step 3, mixing the secondary precipitate with a tungsten source precursor solution, drying, and calcining to obtain an intermediate powder; Step 4, mixing the intermediate powder with the vanadium source precursor solution, the polymer dispersant, the binder, and the pore-forming agent, adjusting the pH value to 7 to 12, and uniformly mixing to form a slurry; Step 5, stamping the slurry obtained in step 4 to obtain corrugated sheets, spraying resin glue between the corrugated sheets and stacking and assembling them to obtain corrugated plate type denitration catalyst blanks, drying and roasting them to obtain corrugated plate type flue gas denitration catalysts.
2. The method for preparing a flue gas denitration catalyst according to claim 1, characterized in that: In step 1, the pH adjusting reagent is ammonia water, and the pH value is adjusted to 7-12; the titanium source precursor solution is calculated as TiO2, and the aluminum source precursor solution is calculated as Al2O3, and the mass ratio of the titanium source precursor solution to the aluminum source precursor solution is 100:0.3-5.
0.
3. The method for preparing a flue gas denitration catalyst according to claim 1, characterized in that: The strong alkaline solution in step 2 is an alkali metal hydroxide solution or an alkaline earth metal hydroxide solution; the tungsten source precursor solution is calculated as tungsten trioxide, the titanium source precursor solution is calculated as TiO2, and the mass ratio of the tungsten source precursor solution to the titanium source precursor solution is 0.5-6.0:100; the mixing method in step 4 is stirring or ultrasonic oscillation, and the mixing time is 0.1-8h; the water mass content of the slurry in step 4 is 5-40%.
4. The method for preparing a flue gas denitration catalyst according to claim 1, characterized in that: The polymer dispersant is at least one of polyethylene glycol, polyacrylamide and polyvinyl pyrrolidone; the binder is at least one of carboxymethyl cellulose and hydroxypropyl cellulose; the pore-forming agent is at least one of polyethylene oxide, polymethyl methacrylate and sesbania powder.
5. The method for preparing a flue gas denitration catalyst according to claim 1, characterized in that: The vanadium source precursor solution is calculated as V2O5, the titanium source precursor solution is calculated as TiO2, and the mass ratio of the vanadium source precursor solution to the titanium source precursor solution is 0.2-5.0:100; the titanium source precursor solution is calculated as TiO2, the mass ratio of the polymer dispersant to the titanium source precursor solution is 0.1-2.0:100, the mass ratio of the binder to the titanium source precursor solution is 0.1-2.0:100, and the mass ratio of the pore former to the titanium source precursor solution is 0.1-2.0:
100.
6. The method for preparing a flue gas denitration catalyst according to claim 1, characterized in that: In step 3 and step 5, the calcination temperature is 450-680° C., and the calcination time is 2-40 hours.
7. The method for preparing a flue gas denitration catalyst according to claim 1, characterized in that: In the step 4, glass fiber is added, the titanium source precursor solution is calculated as TiO2, and the mass ratio of the glass fiber to the titanium source precursor solution is 2 to 10:
100.
8. The method for preparing a flue gas denitration catalyst according to claim 1, characterized in that: In the step 5, the calcination is performed by programmed heating according to the following process: the dried corrugated plate type denitration catalyst blank is heated to a predetermined temperature of 450-680°C, and the heating rate is controlled to be no more than 1°C / min. After the temperature reaches the predetermined temperature, it is calcined at a constant temperature for 2-40 hours, and then cooled at a rate of no more than 4°C / min to below 50°C to obtain a corrugated plate type flue gas denitration catalyst.
9. The method for preparing a flue gas denitration catalyst according to claim 1, characterized in that: The corrugated plate catalyst obtained in step 5 has a corrugated plate thickness of 0.2 to 0.6 mm, a corrugated width of 4 to 8 mm, and a corrugated height of 4 to 10 mm.
10. The flue gas denitration catalyst obtained by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Honeycomb flue gas denitrification catalyst and preparation method thereof
CN103143396B
A method for preparing a honeycomb denitration catalyst with increased specific surface area
CN107096524B
A honeycomb denitrification catalyst with improved strength and its preparation method
CN107138150B
Corrugated plate type denitration catalyst and preparation method thereof
CN111330634A
Honeycomb de-nitration catalyst suitable for high-arsenic fume and preparation method of honeycomb de-nitration catalyst