A non-metallic catalyst for synthesizing cyclic carbonate from CO2 and epoxide, preparation method and application thereof
By heating cyanamide and azo heterocyclic ring with reflux stirring in ethanol and copolymerizing with halogenated benzyl, a metal-free catalyst was prepared, which solved the complex preparation of cyclic carbonate catalysts for the addition of CO2 and epoxide in the prior art. The problems of high cost and limited activity achieve convenient, economical and efficient catalyst preparation and recycling.
Patent Information
- Application Number
- CN202111647328.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-12-29
AI Technical Summary
The catalysts used in the prior art for the synthesis of cyclic carbonates with CO2 and epoxide addition have problems such as complex preparation, high cost, limited catalytic activity and difficulty in recycling, especially metal catalysts that will affect product quality.
Cyanamide or its polymer and C-C anicycline react with reflux and stirring in ethanol to obtain intermediate N-CN, and then copolymerize with halogenated benzyl to prepare a metal-free non-metallic catalyst and pass through the slurry state The bed reactor carries out catalytic reactions under suitable conditions and catalyst recovery is achieved by simple centrifugation or filtration.
It realizes a non-metallic catalyst that is conveniently prepared, low-cost, high catalyst activity and reusable, reduces production costs, avoids metal contamination, and simplifies the catalyst recovery and product separation process.
Smart Images

Figure CN116408119B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of heterogeneous catalysis, and specifically relates to a non-metallic solid catalyst for synthesizing cyclic carbonate by cycloaddition of CO2 and epoxy hydrocarbon in the absence of solvent, a preparation method and application thereof. Background Art
[0002] The large amount of CO2 emissions caused by industrialization is the main cause of the greenhouse effect. CO2 is also a non-toxic, cheap and abundant C1 resource. With the rapid consumption of fossil fuels, the conversion and utilization of CO2 has become one of the hot research topics in the field of industrial catalysis and organic synthesis in recent years. Among them, the process of synthesizing cyclic carbonates through CO2 cycloaddition is one of the most promising pathways for the catalytic conversion of CO2 because of its low raw material price and 100% atomic utilization, which conforms to the development concept of "green chemistry" and "atom economy".
[0003] Propylene carbonate is the most representative compound in the cyclic carbonate series. As an important chemical product, propylene carbonate can be used as a clean polar solvent, polycarbonate synthesis, electrolyte, cosmetic additive, etc. The synthesis of propylene carbonate with CO2 and propylene oxide as raw materials under the action of catalyst has the advantages of green sustainability compared with the traditional phosgene method and oxidative carbonylation method. At present, the catalysts used in this synthesis method include metal halides, ionic liquids and metal complexes. Among them, ionic liquids containing halide ions are considered to be the most active catalysts. However, the reaction system of ionic liquid-catalyzed CO2 and propylene oxide to synthesize propylene carbonate is homogeneous catalysis, which has difficulties such as catalyst recovery and product separation. In contrast, heterogeneous catalysts have significant advantages such as convenient recovery and simple product separation. Currently reported materials for CO2-catalyzed synthesis of propylene carbonate mainly include immobilized ionic liquids, nitrided zeolites, hydrotalcites and other materials. In the long-term catalytic reaction of these materials, the pores are easily blocked, and the active sites of some catalysts will also be dissolved. In view of this, developing a multiphase catalyst with easy recycling and stable structure is the only way to achieve efficient catalytic conversion of CO2 to synthesize propylene carbonate.
[0004] In recent years, graphite carbon nitride (g-C3N4) as a new type of carbonaceous material has attracted widespread attention in the fields of thermal catalysis, photocatalysis, gas storage, semiconductors, etc. In terms of composition and structure, the main unit of g-C3N4 is tris-s-triazine, and there are a large number of amino functional groups at the edge of its graphite-like layer. Therefore, g-C3N4 is a typical solid base material. At present, there are literature reports using g-C3N4 as a catalyst for catalytic Nauwenge condensation, ester exchange and CO2 and epoxide cycloaddition to synthesize cyclic carbonates. Based on the structure and properties of g-C3N4 materials, g-C3N4 is expected to be used to catalyze the cycloaddition reaction of CO2 and epoxides.
[0005] Although g-C3N4 is rich in amino functional groups, most of the nitrogen atoms are highly conjugated on the graphite-like layer, so the alkalinity is very weak); and the content of amino species at the edge of the graphite-like layer is relatively small, so the alkalinity strength of the overall g-C3N4 material is relatively weak. Second, the g-C3N4 synthesized by conventional thermal polymerization has a very low specific surface area (<10m 2 g -1 ), the exposed basic sites of the catalyst are limited. Third, the basic sites of g-C3N4 material can adsorb and activate CO2 molecules, but it is difficult to activate epoxy compounds. Activation of epoxy compounds generally requires metal ions or halide ions. Therefore, the activity of g-C3N4 raw powder in catalyzing CO2 cycloaddition reaction is very limited.
[0006] The solutions reported in the literature mainly involve preparing high specific surface area mesoporous g-C3N4 or introducing halogen (such as bromine-containing ionic liquid) into the g-C3N4 skeleton [Catalysis Science & Technology, 2015, 5, 447–454.; Journal of Molecular Catalysis A: Chemical, 2015, 403, 77–83.]. Although the catalysts obtained by these two methods are very active, the catalyst preparation is complicated and the cost is very high. In particular, mesoporous g-C3N4 materials are basically all prepared by the hard template method, which is not only complicated in preparation process, but also uses a heavily polluted HF solution.
[0007] Huang et al. (Applied Catalysis B, 2013, 136, 269–277) reported that g-C3N4 catalyst supported by SBA-15 can catalyze the cycloaddition reaction of CO2. When the initial CO2 pressure was 3.5 MPa, the reaction temperature was 150 °C and the reaction time was 1 hour, the conversion rate of epoxystyrene was as high as 93%. However, the preparation process of the catalyst is based on the gas phase chemical deposition method of dicyandiamide on the SBA-15 carrier, which is relatively complicated, and the synthesis price of SBA-15 is expensive.
[0008] Xu et al. (Journal of Molecular Catalysis A 2015, 403, 77–83.) reported a ZnCl2 / mp-C3N4 catalyst for CO2 conversion to produce cyclic carbonates, with a cyclic carbonate yield of 72.6%. Patent CN108772088A discloses a gC3N4 catalyst for CO2 cycloaddition to synthesize cyclic carbonates and a preparation method thereof, but the preparation process of the method is complicated, including calcination of precursors to prepare carbon nitride, metal salt solution and alkaline solution such as NaOH, ultrasonic treatment of carbon nitride, mixing of metal salt solution and alkaline solution such as NaOH and carbon nitride, precipitation, hydrothermal aging, washing and drying, calcination, etc., and a single batch of catalyst preparation takes 3-4 days.
[0009] CN112156799A discloses a catalyst for CO2 cycloaddition reaction, its preparation method and application, but N,N-dimethylformamide needs to be added as a co-catalyst during the use of the catalyst, and the co-catalyst is dissolved in the reaction liquid. After the reaction is completed, the co-catalyst must be separated from the product. In addition, metals are added to the catalysts reported and invented above. After the metals enter the carbonate product, the product quality will be affected, especially when used in the battery manufacturing process, the carbonate metal content is required to be high.
[0010] Patent CN105536838A discloses a method for preparing an acid-base bifunctionalized C3N4 catalyst and a cyclic carbonate. The material is synthesized by copolymerization of melamine and a cyclotriphosphazene derivative, and exhibits high catalytic activity for the cycloaddition reaction of CO2. Nevertheless, this method still has some shortcomings: (1) Cyclotriphosphazene derivatives are expensive, resulting in a high catalyst preparation cost. (2) The catalysis requires the use of quaternary ammonium salts such as tetrabutylammonium bromide as a co-catalyst. Therefore, the development of an environmentally friendly heterogeneous catalyst that is easy to prepare has important theoretical and practical significance for the efficient utilization of CO2 and the green synthesis of propylene carbonate.
[0011] Su et al. (Catalysis Science & Technology, 2018, 8, 5582–5593.) used urea to prepare Ug-C3N4 and used it for CO2 conversion to produce cyclic carbonates. Although the initial activity of the reaction was high, the recycling effect was poor and the catalyst was difficult to recycle and reuse. Huang et al. (Catalysis Science and Technology, 2016, 6, 2942–2948) reported H2SO4-modified g-C3N4-S and used it for CO2 conversion to produce cyclic carbonates. However, during the conversion reaction, tetrabutylamine halides, N,N-dimethylformamide and other co-catalysts were required. However, such co-catalysts were easily soluble in the reaction solution, which increased the cost of product separation and purification in the later stage.
[0012] Therefore, it is necessary to provide a convenient non-metallic solid catalyst with high catalytic activity. Summary of the invention
[0013] The technical problem to be solved by the present invention is to provide a metal-free solid non-metal catalyst which is easy to prepare and has high catalytic activity, a preparation method and its application for the reaction of synthesizing cyclic carbonate by addition of CO2 and epoxide.
[0014] To achieve the above object, the present invention provides a method for preparing a non-metallic catalyst for synthesizing cyclic carbonate from CO2 and epoxide, the preparation method comprising the following steps:
[0015] (1) Preparation of intermediate N-CN: After mixing one or more of cyanamide or its polymers with a C-C nitrogen heterocycle, the mixture is refluxed, stirred and heated in ethanol to obtain a solid, and the obtained solid is dried and calcined under an inert gas atmosphere to obtain the intermediate N-CN;
[0016] (2) Preparation of non-metallic catalyst: The intermediate N-CN is mixed with the halogenated benzyl, and copolymerization reaction is carried out in a reaction medium. The product is filtered, washed and dried to obtain a non-metallic catalyst.
[0017] In the preparation method of the present invention, in step (1), cyanamide or its polymer is not particularly limited. Preferably, cyanamide or its polymer is one or more of cyanamide, dicyandiamide and melamine, and dicyandiamide or melamine is most preferred.
[0018] In the preparation method of the present invention, in step (1), the nitrogen heterocycle of C~C is not particularly limited. Preferably, the nitrogen heterocycle of C~C is one or more of 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), 1,5-diazabicyclo[4.3.0]-5-nonene (DBN), 4-dimethylaminopyridine (DMAP) or 1,4-diazidebicyclo[2.2.2]octane (DABCO), preferably DBU, DMAP and DABCO.
[0019] In the preparation method of the present invention, in step (1), the mass ratio of cyanamide or its polymer to C-C nitrogen heterocycle is 1:1-10:1, preferably 3:1-10:1.
[0020] In the preparation method of the present invention, in step (1), the inert gas is nitrogen, helium, or argon, preferably nitrogen.
[0021] In the preparation method of the present invention, in step (1), the temperature of the reflux stirring heating reaction is 60-120°C, preferably 80-100°C.
[0022] In the preparation method of the present invention, in step (1), the reflux stirring heating reaction time is 2-24 hours, preferably 6-18 hours.
[0023] In the preparation method of the present invention, in step (1), the calcination temperature is 300-600°C, preferably 400-550°C.
[0024] In the preparation method of the present invention, in step (1), the calcination time is 1-12 hours, preferably 4-6 hours.
[0025] In the preparation method of the present invention, in step (2), the halogenated benzyl is at least one of benzyl bromide and benzyl chloride, preferably benzyl bromide.
[0026] In the preparation method of the present invention, in step (2), the reaction medium is at least one of methanol, ethanol and toluene, preferably toluene.
[0027] In the preparation method of the present invention, in step (2), the mass ratio of the intermediate N-CN to the halogenated benzyl in the copolymerization reaction is 1:1-10:1, preferably 1.5:1-5:1.
[0028] In the preparation method of the present invention, in step (2), the temperature of the copolymerization reaction is 60-120°C, preferably 80-100°C.
[0029] In the preparation method of the present invention, in step (2), the heating time of the copolymerization reaction is 4-24 hours, preferably 6-12 hours.
[0030] The present invention also provides a non-metallic catalyst obtained by the preparation method of the non-metallic catalyst for synthesizing cyclic carbonate from CO2 and epoxide, wherein no metal component is added during the preparation process of the non-metallic catalyst.
[0031] The present invention further provides an application of the non-metallic catalyst obtained by the above preparation method in the reaction of synthesizing cyclic carbonates from CO2 and epoxide. The reaction comprises: adding epoxide and the non-metallic catalyst into a reactor, charging CO2 gas to adjust the reaction pressure, heating and reacting.
[0032] The application of the present invention does not particularly limit the addition ratio of the catalyst to the epoxide to 1:(10-160) g / g, and is preferably 1:(50-100) g / g.
[0033] The application of the present invention is not particularly limited to epoxides. Preferably, the epoxide is at least one of propylene oxide, ethylene oxide, chloroethylene oxide and styrene oxide.
[0034] The application of the present invention is not particularly limited to the pressure of the CO2 gas charged to adjust the reaction. Preferably, the pressure is 0.05-5MPa, and most preferably 1.0-3.0MPa.
[0035] The application of the present invention is not particularly limited to the reaction temperature. Preferably, the temperature is 70-240°C, and most preferably 120-160°C.
[0036] The application of the present invention does not particularly limit the reaction time. Preferably, the reaction time is 2-20 hours, and most preferably, 3-8 hours.
[0037] The application of the present invention is not particularly limited to the type of reactor, and is preferably applicable to a slurry bed reactor.
[0038] Compared with homogeneous catalysts such as ionic liquids and metal complexes in the prior art, the present invention has the advantages of convenient preparation, low cost and convenient catalyst recovery. After the non-metallic catalyst of the present invention is recycled and reused many times, the yield of cyclic carbonate does not change significantly, proving that the non-metallic catalyst of the present invention has the advantage of good reusability, thereby greatly reducing production costs.
[0039] In addition, after the reaction of the non-metallic catalyst of the present invention is completed, the reaction system can be simply centrifuged or filtered to achieve catalyst recovery and product separation. The catalyst component of the present invention does not contain any metal components, and will not cause metal pollution to the product of the catalytic reaction; in the catalytic reaction, there is no need to add co-catalysts such as tetrabutylamine halide and N,N-dimethylformamide, thereby reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The present invention is a schematic diagram of the preparation process of the non-metal catalyst for synthesizing cyclic carbonate from CO2 and epoxide in a slurry bed reactor. DETAILED DESCRIPTION
[0041] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.
[0042] Example 1
[0043] (1) Preparation of non-metallic catalysts
[0044] In a single-necked flask, add 6 g of dicyandiamide, 2 g of DBU and 100 g of ethanol. Install a condenser with water circulation on the flask, and reflux and stir at 80°C for 12 hours. Then separate the solid-liquid mixture by centrifugation or filtration to obtain solid A1.
[0045] The solid A1 was fully dried in an oven, placed in a quartz boat, and then placed in a tube furnace. It was heated from room temperature to 450°C at a heating rate of 1-3°C / min under a nitrogen atmosphere and maintained at this temperature for 4 hours. The obtained material was recorded as intermediate N-CN-1;
[0046] The obtained intermediate N-CN-1 and benzyl bromide are added to a single-necked flask in a ratio of 2:1, and then 100 mL of toluene is added. The flask is equipped with a water circulation condenser and refluxed and stirred at a heating temperature of 80°C for 10 hours. The solid-liquid mixture is then separated by centrifugation or filtration to obtain solid B1. The obtained solid B1 is added to 20 mL of toluene, and stirring and washing are continued at room temperature for 4 hours. After centrifugation or filtration separation again, it is fully dried in a vacuum oven to obtain a catalyst, and the catalyst material is recorded as BrN-CN-1.
[0047] (2) Catalytic reaction
[0048] In a 50mL slurry bed reactor, add 0.2g of catalyst and 10g of propylene oxide. Charge the reactor with CO2 (purity exceeding 99.9%) until the pressure reaches 1.0MPa, then slowly open the vent valve to evacuate the CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, then charge the reactor with CO2 to a pressure of 2.0MPa. Start stirring and react at a reaction temperature of 160°C for 8 hours.
[0049] (3) Catalyst recovery and product separation
[0050] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0051] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0052] (4) Product analysis
[0053] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0054] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was 89%.
[0055] Example 2
[0056] (1) Preparation of non-metallic catalysts
[0057] In a single-necked flask, add 6 g of dicyandiamide, 1 g of DMAP and 100 g of ethanol. Install a condenser with water circulation on the flask, and reflux and stir at 100°C for 18 hours. Then separate the solid-liquid mixture by centrifugation or filtration to obtain solid A2.
[0058] The solid A2 was fully dried in an oven, placed in a quartz boat, and then placed in a tube furnace. It was heated from room temperature to 500°C at a heating rate of 1-3°C / min under a nitrogen atmosphere and maintained at this temperature for 5 hours. The obtained material was recorded as intermediate N-CN-2;
[0059] The obtained intermediate N-CN-2 and benzyl bromide are added to a single-necked flask in a ratio of 1.5:1, and then 100 mL of ethanol is added. The flask is equipped with a water circulation condenser and refluxed and stirred at a heating temperature of 100°C for 8 hours. The solid-liquid mixture is then separated by centrifugation or filtration to obtain solid B2. The obtained solid B2 is added to 20 mL of toluene, and continued to be stirred and washed at room temperature for 4 hours. After centrifugation or filtration separation again, it is fully dried in a vacuum oven to obtain a catalyst, and the catalyst material is recorded as BrN-CN-2.
[0060] (2) Catalytic reaction
[0061] In a 50mL slurry bed reactor, add 0.2g of catalyst and 10g of styrene oxide. Charge the reactor with CO2 (purity exceeding 99.9%) until the pressure reaches 1.0MPa, then slowly open the vent valve to evacuate the CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, then charge the reactor with CO2 to a pressure of 2.5MPa. Start stirring and react at a reaction temperature of 140°C for 4 hours.
[0062] (3) Catalyst recovery and product separation
[0063] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0064] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0065] (4) Product analysis
[0066] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0067] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was 92%.
[0068] Example 3
[0069] (1) Preparation of non-metallic catalysts
[0070] In a single-necked flask, add 4 g of melamine, 0.4 g of DMAP and 100 g of ethanol. Install a condenser for water circulation on the flask, and reflux and stir at 90°C for 6 hours. Then separate the solid-liquid mixture by centrifugation or filtration to obtain solid A3.
[0071] The solid A3 was fully dried in an oven, placed in a quartz boat, and then placed in a tube furnace. It was heated from room temperature to 400°C at a heating rate of 1-3°C / min under a nitrogen atmosphere and maintained at this temperature for 6 hours. The obtained material was recorded as intermediate N-CN-3;
[0072] The obtained intermediate N-CN-3 and benzyl chloride are added to a single-necked flask in a ratio of 2.5:1, and then 100 mL of methanol is added. The flask is equipped with a water circulation condenser and refluxed and stirred at a heating temperature of 90°C for 12 hours. The solid-liquid mixture is then separated by centrifugation or filtration to obtain solid B3. The obtained solid B3 is added to 20 mL of toluene, and stirring and washing are continued at room temperature for 4 hours. After centrifugation or filtration separation again, it is fully dried in a vacuum oven to obtain a catalyst, and the catalyst material is recorded as ClN-CN-3.
[0073] (2) Catalytic reaction
[0074] In a 50mL slurry bed reactor, add 0.3g of catalyst and 15g of chloroethylene oxide. Charge the reactor with CO2 (purity exceeding 99.9%) until the pressure is 1.0MPa, then slowly open the vent valve to evacuate the CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, and then charge the reactor with CO2 to a pressure of 1.0MPa. Start stirring and react at a reaction temperature of 160°C for 7 hours.
[0075] (3) Catalyst recovery and product separation
[0076] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0077] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0078] (4) Product analysis
[0079] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0080] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was 93%.
[0081] Example 4
[0082] (1) Preparation of non-metallic catalysts
[0083] In a single-necked flask, add 4 g of melamine, 0.5 g of DABCO and 100 g of ethanol. Install a condenser for water circulation on the flask, and reflux and stir at 100°C for 10 hours. Then separate the solid-liquid mixture by centrifugation or filtration to obtain solid A4.
[0084] The solid A4 was fully dried in an oven, placed in a quartz boat, and then placed in a tube furnace. It was heated from room temperature to 550°C at a heating rate of 1-3°C / min under a nitrogen atmosphere and maintained at this temperature for 5 hours. The obtained material was recorded as intermediate N-CN-4;
[0085] The obtained intermediate N-CN-4 and benzyl chloride are added to a single-necked flask in a ratio of 3:1, and then 100 mL of toluene is added. The flask is equipped with a water circulation condenser and refluxed and stirred at a heating temperature of 100°C for 9 hours. The solid-liquid mixture is then separated by centrifugation or filtration to obtain solid B4. The obtained solid B4 is added to 20 mL of toluene, and stirring and washing are continued at room temperature for 4 hours. After centrifugation or filtration separation again, it is fully dried in a vacuum oven to obtain a catalyst, and the catalyst material is recorded as ClN-CN-4.
[0086] (2) Catalytic reaction
[0087] In a 50mL slurry bed reactor, add 0.2g of catalyst and 20g of propylene oxide. Charge the reactor with CO2 (purity exceeding 99.9%) until the pressure reaches 1.0MPa, then slowly open the vent valve to evacuate the CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, then charge the reactor with CO2 to a pressure of 3.0MPa. Start stirring and react at a reaction temperature of 120°C for 6 hours.
[0088] (3) Catalyst recovery and product separation
[0089] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0090] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0091] (4) Product analysis
[0092] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0093] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was 88%.
[0094] Example 5
[0095] (1) Preparation of non-metallic catalysts
[0096] In a single-necked flask, add 4 g of dicyandiamide, 0.5 g of DMAP and 100 g of ethanol. Install a condenser with water circulation on the flask, and reflux and stir at 80°C for 7 hours. Then separate the solid-liquid mixture by centrifugation or filtration to obtain solid A5.
[0097] The solid A5 was fully dried in an oven, placed in a quartz boat, and then placed in a tube furnace. It was heated from room temperature to 525°C at a heating rate of 1-3°C / min under a nitrogen atmosphere and maintained at this temperature for 5 hours. The obtained material was recorded as intermediate N-CN-5;
[0098] The obtained intermediate N-CN-5 and benzyl bromide are added to a single-necked flask in a ratio of 5:1, and then 100 mL of toluene is added. The flask is equipped with a water circulation condenser and refluxed and stirred at a heating temperature of 90°C for 6 hours. The solid-liquid mixture is then separated by centrifugation or filtration to obtain solid B5. The obtained solid B5 is added to 20 mL of toluene, and stirring and washing are continued at room temperature for 4 hours. After centrifugation or filtration separation again, it is fully dried in a vacuum oven to obtain a catalyst, and the catalyst material is recorded as BrN-CN-5.
[0099] (2) Catalytic reaction
[0100] In a 50mL slurry bed reactor, add 0.2g of catalyst and 15g of styrene oxide. Charge the reactor with CO2 (purity exceeding 99.9%) until the pressure reaches 1.0MPa, then slowly open the vent valve to evacuate the CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, then charge the reactor with CO2 to a pressure of 2.0MPa. Start stirring and react at a reaction temperature of 150°C for 3 hours.
[0101] (3) Catalyst recovery and product separation
[0102] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0103] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0104] (4) Product analysis
[0105] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0106] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was 93%.
[0107] Example 6
[0108] (1) Preparation of non-metallic catalysts
[0109] In a single-necked flask, add 4 g of dicyandiamide, 0.4 g of DBU and 100 g of ethanol. Install a condenser with water circulation on the flask, and reflux and stir at 90°C for 12 hours. Then separate the solid-liquid mixture by centrifugation or filtration to obtain solid A6.
[0110] The solid A6 was fully dried in an oven, placed in a quartz boat, and then placed in a tube furnace. It was heated from room temperature to 500°C at a heating rate of 1-3°C / min under an argon atmosphere and maintained at this temperature for 4 hours. The obtained material was recorded as intermediate N-CN-6;
[0111] The obtained intermediate N-CN-6 and benzyl bromide are added to a single-necked flask in a ratio of 4.5:1, and then 100 mL of toluene is added. The flask is equipped with a water circulation condenser and refluxed and stirred at a heating temperature of 100°C for 7 hours. The solid-liquid mixture is then separated by centrifugation or filtration to obtain solid B6. The obtained solid B6 is added to 20 mL of toluene, and stirring and washing are continued at room temperature for 4 hours. After centrifugation or filtration separation again, it is fully dried in a vacuum oven to obtain a catalyst, and the catalyst material is recorded as BrN-CN-6.
[0112] (2) Catalytic reaction
[0113] In a 50mL slurry bed reactor, add 0.2g of catalyst and 10g of chloroethylene oxide. Charge the reactor with CO2 (purity exceeding 99.9%) until the pressure reaches 1.0MPa, then slowly open the vent valve to evacuate the CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, then charge the reactor with CO2 to a pressure of 2.0MPa. Start stirring and react at a reaction temperature of 140°C for 6 hours.
[0114] (3) Catalyst recovery and product separation
[0115] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0116] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0117] (4) Product analysis
[0118] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0119] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was 92%.
[0120] Example 7
[0121] (1) Preparation of non-metallic catalysts
[0122] In a single-necked flask, add 6 g of melamine, 0.67 g of DBU and 100 g of ethanol. The flask is equipped with a condenser for water circulation, and refluxed and stirred at 100°C for 16 hours. The solid-liquid mixture is then separated by centrifugation or filtration to obtain solid A7.
[0123] The solid A7 was fully dried in an oven, placed in a quartz boat, and then placed in a tube furnace. It was heated from room temperature to 550°C at a heating rate of 1-3°C / min in a helium atmosphere and maintained at this temperature for 4 hours. The obtained material was recorded as intermediate N-CN-7;
[0124] The obtained solid and benzyl bromide are added to a single-necked flask in a ratio of 1.5:1, and then 100 mL of toluene is added. The flask is equipped with a water circulation condenser and refluxed and stirred at a heating temperature of 80°C for 11 hours. The solid-liquid mixture is then separated by centrifugation or filtration to obtain solid B7. The obtained solid B7 is added to 20 mL of toluene, and stirring and washing are continued at room temperature for 4 hours. After centrifugation or filtration separation again, it is fully dried in a vacuum oven to obtain a catalyst, and the catalyst material is recorded as BrN-CN-7.
[0125] (2) Catalytic reaction
[0126] In a 50mL slurry bed reactor, add 0.2g of catalyst and 15g of propylene oxide. Charge the reactor with CO2 (purity exceeding 99.9%) until the pressure reaches 1.0MPa, then slowly open the vent valve to evacuate the CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, then charge the reactor with CO2 to a pressure of 2.5MPa. Start stirring and react at a reaction temperature of 130°C for 7 hours.
[0127] (3) Catalyst recovery and product separation
[0128] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0129] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0130] (4) Product analysis
[0131] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0132] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was 90%.
[0133] Example 8
[0134] (1) Preparation of non-metallic catalysts
[0135] In a single-necked flask, add 6 g of dicyandiamide, 1.5 g of DBU and 100 g of ethanol. Install a condenser with water circulation on the flask, and reflux and stir at 80°C for 10 hours. Then separate the solid-liquid mixture by centrifugation or filtration to obtain solid A8.
[0136] The solid A8 was fully dried in an oven, placed in a quartz boat, and then placed in a tube furnace. It was heated from room temperature to 475°C at a heating rate of 1-3°C / min under a nitrogen atmosphere and maintained at this temperature for 5 hours. The obtained material was recorded as intermediate N-CN-8;
[0137] The obtained intermediate N-CN-8 and benzyl chloride are added to a single-necked flask in a ratio of 4:1, and then 100 mL of toluene is added. The flask is equipped with a water circulation condenser and refluxed and stirred at a heating temperature of 100°C for 10 hours. The solid-liquid mixture is then separated by centrifugation or filtration to obtain solid B8. The obtained solid B8 is added to 20 mL of toluene, and stirring and washing are continued at room temperature for 4 hours. After centrifugation or filtration separation again, it is fully dried in a vacuum oven to obtain a catalyst, and the catalyst material is recorded as ClN-CN-8.
[0138] (2) Catalytic reaction
[0139] In a 50mL slurry bed reactor, add 0.2g of catalyst and 10g of propylene oxide. Charge the reactor with CO2 (purity exceeding 99.9%) until the pressure reaches 1.0MPa, then slowly open the vent valve to evacuate the CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, then charge the reactor with CO2 to a pressure of 3.0MPa. Start stirring and react at a reaction temperature of 120°C for 8 hours.
[0140] (3) Catalyst recovery and product separation
[0141] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0142] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0143] (4) Product analysis
[0144] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0145] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was 92%.
[0146] Example 9
[0147] (1) Preparation of non-metallic catalysts
[0148] In a single-necked flask, add 6 g of dicyandiamide, 1 g of DABCO and 100 g of ethanol. Install a water-circulating condenser on the flask and reflux and stir at 90°C for 6 hours. Then separate the solid-liquid mixture by centrifugation or filtration to obtain solid A9.
[0149] The solid A9 was fully dried in an oven, placed in a quartz boat, and then placed in a tube furnace. It was heated from room temperature to 425°C at a heating rate of 1-3°C / min under an argon atmosphere and maintained at this temperature for 6 hours. The obtained material was recorded as intermediate N-CN-9;
[0150] The obtained intermediate N-CN-9 and benzyl bromide are added to a single-necked flask in a ratio of 2.5:1, and then 100 mL of toluene is added. The flask is equipped with a water circulation condenser and refluxed and stirred at a heating temperature of 90°C for 9 hours. The solid-liquid mixture is then separated by centrifugation or filtration to obtain solid B9. The obtained solid B9 is added to 20 mL of toluene, and stirring and washing are continued at room temperature for 4 hours. After centrifugation or filtration separation again, it is fully dried in a vacuum oven to obtain a catalyst, and the catalyst material is recorded as BrN-CN-9.
[0151] (2) Catalytic reaction
[0152] In a 50mL slurry bed reactor, add 0.2g of catalyst and 15g of propylene oxide. Charge the reactor with CO2 (purity exceeding 99.9%) until the pressure reaches 1.0MPa, then slowly open the vent valve to evacuate the CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, then charge the reactor with CO2 to a pressure of 1.5MPa. Start stirring and react at a reaction temperature of 150°C for 5 hours.
[0153] (3) Catalyst recovery and product separation
[0154] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0155] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0156] (4) Product analysis
[0157] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0158] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was 91%.
[0159] Example 10
[0160] (1) Preparation of non-metallic catalysts
[0161] In a single-necked flask, add 5 g of dicyandiamide, 1 g of DBU and 80 g of ethanol. Install a condenser with water circulation on the flask, and reflux and stir at 90°C for 16 hours. Then separate the solid-liquid mixture by centrifugation or filtration to obtain solid A10.
[0162] The solid A10 was fully dried in an oven, placed in a quartz boat, and then placed in a tube furnace. It was heated from room temperature to 430°C at a heating rate of 1-3°C / min in a helium atmosphere and maintained at this temperature for 4 hours. The obtained material was recorded as intermediate N-CN-10;
[0163] The obtained intermediate N-CN-1 and benzyl bromide are added to a single-necked flask in a ratio of 1:1, and then 100 mL of toluene is added. The flask is equipped with a water circulation condenser and refluxed and stirred at a heating temperature of 80°C for 10 hours. The solid-liquid mixture is then separated by centrifugation or filtration to obtain solid B10. The obtained solid B10 is added to 20 mL of toluene, and stirring and washing are continued at room temperature for 4 hours. After centrifugation or filtration separation again, it is fully dried in a vacuum oven to obtain a catalyst, and the catalyst material is recorded as BrN-CN-10.
[0164] (2) Catalytic reaction
[0165] In a 50mL slurry bed reactor, add 0.2g of catalyst and 2g of propylene oxide. Charge the reactor with CO2 (purity exceeding 99.9%) until the pressure reaches 1.0MPa, then slowly open the vent valve to evacuate the CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, then charge the reactor with CO2 to a pressure of 2.2MPa. Start stirring and react at a reaction temperature of 150°C for 8 hours.
[0166] (3) Catalyst recovery and product separation
[0167] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0168] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0169] (4) Product analysis
[0170] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0171] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was 90%.
[0172] Embodiment 11
[0173] (1) Preparation of non-metallic catalysts
[0174] In a single-necked flask, add 4 g of cyanamide, 2 g of DBN and 100 g of ethanol. Install a condenser with water circulation on the flask, and reflux and stir at 80°C for 12 hours. Then separate the solid-liquid mixture by centrifugation or filtration to obtain solid A11.
[0175] The solid A11 was fully dried in an oven, placed in a quartz boat, and then placed in a tube furnace. It was heated from room temperature to 525°C at a heating rate of 1-3°C / min under a nitrogen atmosphere and maintained at this temperature for 4 hours. The obtained material was recorded as intermediate N-CN-11;
[0176] The obtained intermediate N-CN-11 and benzyl bromide are added to a single-necked flask in a ratio of 10:1, and then 100 mL of ethanol is added. The flask is equipped with a water circulation condenser and refluxed and stirred at a heating temperature of 80°C for 12 hours. The solid-liquid mixture is then separated by centrifugation or filtration to obtain solid B11. The obtained solid B11 is added to 20 mL of ethanol, and stirring and washing are continued at room temperature for 4 hours. After centrifugation or filtration separation again, it is fully dried in a vacuum oven to obtain a catalyst, and the catalyst material is recorded as BrN-CN-11.
[0177] (2) Catalytic reaction
[0178] In a 50mL slurry bed reactor, add 0.2g of catalyst and 32g of chloroethylene oxide. Charge the reactor with CO2 (purity exceeding 99.9%) until the pressure is 1.0MPa, then slowly open the vent valve to evacuate the CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, and then charge the reactor with CO2 to a pressure of 2.5MPa. Start stirring and react at a reaction temperature of 160°C for 18 hours.
[0179] (3) Catalyst recovery and product separation
[0180] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0181] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0182] (4) Product analysis
[0183] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0184] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was 88%.
[0185] Example 12
[0186] (1) Preparation of non-metallic catalysts
[0187] In a single-necked flask, add 6 g of cyanamide, 1 g of DMAP and 90 g of ethanol. Install a condenser with water circulation on the flask, and reflux and stir at 90°C for 18 hours. Then separate the solid-liquid mixture by centrifugation or filtration to obtain solid A12.
[0188] The solid A1 was fully dried in an oven, placed in a quartz boat, and then placed in a tube furnace. It was heated from room temperature to 400°C at a heating rate of 1-3°C / min under an argon atmosphere and maintained at this temperature for 12 hours. The obtained material was recorded as intermediate N-CN-12;
[0189] The obtained intermediate N-CN-12 and benzyl bromide are added to a single-necked flask in a ratio of 10:1, and then 100 mL of methanol is added. The flask is equipped with a water circulation condenser and refluxed and stirred at a heating temperature of 85°C for 12 hours. The solid-liquid mixture is then separated by centrifugation or filtration to obtain solid B12. The obtained solid B12 is added to 20 mL of methanol, and continued to be stirred and washed at room temperature for 4 hours. After centrifugation or filtration separation again, it is fully dried in a vacuum oven to obtain a catalyst, and the catalyst material is recorded as BrN-CN-12.
[0190] (2) Catalytic reaction
[0191] In a 50mL slurry bed reactor, add 0.4g of catalyst and 25g of ethylene oxide. Charge CO2 (purity exceeding 99.9%) into the reactor until the pressure reaches 1.0MPa, then slowly open the vent valve to evacuate CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, then charge CO2 into the reactor until the pressure reaches 3.0MPa. Start stirring, and react at a reaction temperature of 150°C for 8 hours.
[0192] (3) Catalyst recovery and product separation
[0193] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0194] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0195] (4) Product analysis
[0196] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0197] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was 92%.
[0198] Table 1 shows the reuse of the catalyst of Example 2. After each catalytic reaction, the catalyst was washed with ethanol and water and dried, and its catalytic performance was tested under the same conditions. As can be seen from the table, the catalyst can maintain a yield of cyclic propylene carbonate of about 89% after being reused 8 times, which shows that the non-metallic catalyst of the present invention has good reuse performance.
[0199] Table 1 Reuse of non-metallic catalysts
[0200]
[0201]
[0202] Comparative Example 1
[0203] (1) Preparation of non-metallic catalysts
[0204] 15 g of urea was added to a crucible and calcined at 550 ° C in a muffle furnace for 3 hours. After cooling, it was washed with 1 mol / L hydrochloric acid and deionized water respectively to remove the ammonia species on the surface. After filtering, it was dried at 80 ° C for 12 hours. The dried powder was calcined at 400 ° C for 3 hours to obtain Ug-C3N4 catalyst.
[0205] (2) Catalytic reaction
[0206] In a 50mL slurry bed reactor, add 0.2g of catalyst and 10g of propylene oxide. Charge the reactor with CO2 (purity exceeding 99.9%) until the pressure reaches 1.0MPa, then slowly open the vent valve to evacuate the CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, then charge the reactor with CO2 to a pressure of 2.0MPa. Start stirring and react at a reaction temperature of 160°C for 8 hours.
[0207] (3) Catalyst and product separation
[0208] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0209] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0210] (4) Product analysis
[0211] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0212] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was less than 87%.
[0213] Table 2 shows the reuse of the catalyst in Comparative Example 1. After each catalytic reaction, the catalyst was washed with ethanol and water and dried, and its catalytic performance was tested under the same conditions. As can be seen from the table, the yield of cyclic propylene carbonate decreased to 53% after 8 times of reuse. Therefore, the non-metallic catalyst prepared in Comparative Example 1 has poor reuse performance, which will cause higher costs for actual production.
[0214] Table 2 Reuse of catalyst
[0215] Number of times of reuse Cyclic propylene carbonate yield (%) 0 87 1 85 2 79 3 71 4 65 5 63 6 59 7 55 8 53
[0216] Comparative Example 2
[0217] (1) Preparation of non-metallic catalysts
[0218] In a single-necked flask, add 6 g of dicyandiamide and 100 g of ethanol. Install a condenser with water circulation on the flask, and reflux and stir at 80°C for 12 hours. Then separate the solid-liquid mixture by centrifugation or filtration to obtain solid A / 1.
[0219] The solid A / 1 was fully dried in an oven, placed in a quartz boat, and then placed in a tube furnace. It was heated from room temperature to 450°C at a heating rate of 1-3°C / min under a nitrogen atmosphere and maintained at this temperature for 4 hours. The obtained material was recorded as intermediate N-CN- / 1;
[0220] The obtained intermediate N-CN- / 1 and benzyl bromide are added to a single-necked flask in a ratio of 2:1, and then 100 mL of toluene is added. The flask is equipped with a water circulation condenser and refluxed and stirred at a heating temperature of 80°C for 10 hours. The solid-liquid mixture is then separated by centrifugation or filtration to obtain solid B / 1. The obtained solid B / 1 is added to 20 mL of toluene, and stirring and washing are continued at room temperature for 4 hours. After centrifugation or filtration separation again, it is fully dried in a vacuum oven to obtain a catalyst, and the catalyst material is recorded as BrN-CN- / 1.
[0221] (2) Catalytic reaction
[0222] In a 50mL slurry bed reactor, add 0.2g of catalyst and 10g of propylene oxide. Charge the reactor with CO2 (purity exceeding 99.9%) until the pressure reaches 1.0MPa, then slowly open the vent valve to evacuate the CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, then charge the reactor with CO2 to a pressure of 2.0MPa. Start stirring and react at a reaction temperature of 160°C for 8 hours.
[0223] (3) Catalyst recovery and product separation
[0224] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0225] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0226] (4) Product analysis
[0227] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0228] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was 23%.
[0229] In this comparative example, no nitrogen heterocycle was added during the catalyst preparation process. Compared with Example 1, under the same catalyst conditions, the yield of cyclic carbonate in the finally prepared catalyst was very low. The reason is that the catalyst component lacks active sites formed by the copolymerization of nitrogen heterocycles.
[0230] Comparative Example 3
[0231] (1) Preparation of non-metallic catalysts
[0232] In a single-necked flask, add 6 g of dicyandiamide, 2 g of DBU and 100 g of ethanol. Install a condenser with water circulation on the flask, and reflux and stir at 80°C for 12 hours. Then separate the solid-liquid mixture by centrifugation or filtration to obtain solid A / 2.
[0233] The solid A / 2 was fully dried in an oven, placed in a quartz boat, and then placed in a tube furnace. It was heated from room temperature to 450°C at a heating rate of 1-3°C / min under a nitrogen atmosphere and maintained at this temperature for 4 hours. The obtained material was recorded as N-CN- / 2;
[0234] (2) Catalytic reaction
[0235] In a 50mL slurry bed reactor, add 0.2g of catalyst (N-CN- / 2) and 10g of propylene oxide. Charge the reactor with CO2 (purity exceeding 99.9%) until the pressure reaches 1.0MPa, then slowly open the vent valve to evacuate CO2 to replace the air in the reactor. Repeat the above gas replacement operation 3 times, then charge the reactor with CO2 to a pressure of 2.0MPa. Start stirring and react at a reaction temperature of 160°C for 8 hours.
[0236] (3) Catalyst recovery and product separation
[0237] After the catalytic reaction is completed, the reactor is quickly cooled to room temperature. The vent valve is slowly opened to exhaust the gas therein. The mixture of reaction liquid and catalyst in the reactor is taken out, and the catalyst and reaction liquid are separated by centrifugation or filtration.
[0238] The separated catalyst was washed with 20 mL of ethanol for 30 minutes and then filtered. After repeating the above steps 3 times, the filtered catalyst was placed in a vacuum oven and heated at 60° C. for 4 hours under vacuum conditions to obtain a recovered catalyst.
[0239] (4) Product analysis
[0240] The gas chromatograph uses nitrogen as carrier gas, and is equipped with a 30m long SE-54 capillary column and a hydrogen ion flame detector (FID). The temperature of the vaporizer and detector is 250°C. The column box heating program is as follows: keep at 60°C for 3 minutes, then heat to 180°C at a heating rate of 20°C / min, and continue to maintain for 1 minute.
[0241] The product was analyzed by gas chromatography, and the yield of cyclic carbonate was 17%.
[0242] This comparative example lacks the reaction with halogenated aromatic hydrocarbons during the catalyst preparation process. Compared with Example 1, the yield of cyclic carbonate in the finally prepared catalyst is very low under the same catalyst conditions. The reason is that there is a lack of halogen active sites in the catalyst component.
[0243] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A method for preparing a non-metallic catalyst for synthesizing cyclic carbonates from CO2 and epoxides, characterized in that: The preparation method comprises the following steps: (1) Preparation of intermediate N-CN: After mixing one or more of cyanamide or its polymers with a C-C nitrogen heterocycle, the mixture is refluxed, stirred and heated in ethanol to obtain a solid, and the obtained solid is dried and calcined under an inert atmosphere to obtain the intermediate N-CN; (2) Preparation of non-metallic catalyst: The intermediate N-CN is mixed with the halogenated benzyl, and copolymerization reaction is carried out in a reaction medium. The product is filtered, washed and dried to obtain a non-metallic catalyst.
2. The preparation method according to claim 1, characterized in that: In step (1), the polymer of cyanamide is one or more of dicyandiamide and melamine.
3. The preparation method according to claim 2, characterized in that: In step (1), the polymer of cyanamide is dicyandiamide or melamine.
4. The preparation method according to claim 1, characterized in that: In step (1), the C~C nitrogen heterocycle is one or more of 1,8-diazabicyclo[5.4.0]undec-7-ene, 1,5-diazabicyclo[4.3.0]-5-nonene, 4-dimethylaminopyridine or 1,4-diazidebicyclo[2.2.2]octane.
5. The preparation method according to claim 4, characterized in that: In step (1), the C~C nitrogen heterocycle is 1,8-diazabicyclo[5.4.0]undec-7-ene, 4-dimethylaminopyridine and 1,4-diazidebicyclo[2.2.2]octane.
6. The preparation method according to claim 1, characterized in that: In step (1), the mass ratio of the cyanamide or its polymer to the C-C nitrogen heterocycle is 1:1-10:
1.
7. The preparation method according to claim 6, characterized in that: In step (1), the mass ratio of the cyanamide or its polymer to the C-C nitrogen heterocycle is 3:1-10:
1.
8. The preparation method according to claim 1, characterized in that: In step (1), the gas used in the inert atmosphere is nitrogen, helium or argon.
9. The preparation method according to claim 8, characterized in that: In step (1), the gas used in the inert atmosphere is nitrogen.
10. The preparation method according to claim 1, characterized in that: In step (1), the temperature of the reflux stirring heating reaction is 60-120°C and the time is 2-24 hours; the temperature of the calcination is 300-600°C and the time is 1-12 hours.
11. The preparation method according to claim 10, characterized in that: In step (1), the temperature of the reflux stirring heating reaction is 80-100°C and the time is 6-18 hours; the temperature of the calcination is 400-550°C and the time is 4-6 hours.
12. The preparation method according to claim 1, characterized in that: In step (2), the halogenated benzyl is at least one of benzyl bromide and benzyl chloride; and the reaction medium is at least one of methanol, ethanol and toluene.
13. The preparation method according to claim 1, characterized in that: In step (2), the halogenated benzyl is benzyl bromide.
14. The preparation method according to claim 1, characterized in that: In step (2), the reaction medium is toluene.
15. The preparation method according to claim 1, characterized in that: In step (2), the mass ratio of the intermediate N-CN to the halogenated benzyl in the copolymerization reaction is 1:1-10:
1.
16. The preparation method according to claim 15, characterized in that: In step (2), the mass ratio of the intermediate N-CN to the halogenated benzyl in the copolymerization reaction is 1.5:1-5:
1.
17. The preparation method according to claim 1, characterized in that: In step (2), the copolymerization reaction is carried out at a temperature of 60-120° C. and for a time of 4-24 hours.
18. The preparation method according to claim 17, characterized in that: In step (2), the copolymerization reaction is carried out at a temperature of 80-100° C. and for a time of 6-12 hours.
19. A non-metallic catalyst obtained by the method for preparing a non-metallic catalyst for synthesizing cyclic carbonate from CO2 and epoxide according to any one of claims 1 to 18.
20. Use of a non-metallic catalyst obtained by the preparation method according to any one of claims 1 to 18 in the reaction of synthesizing cyclic carbonates from CO2 and epoxides, characterized in that: The reaction comprises: adding epoxide and non-metal catalyst into a reactor, charging CO2 gas to adjust the reaction pressure, heating and reacting.
21. The use according to claim 20, characterized in that The addition ratio of the non-metallic catalyst and the epoxide is 1:(10-160) g / g; the epoxide is at least one of propylene oxide, ethylene oxide, chloroethylene oxide and styrene oxide.
22. The use according to claim 20, characterized in that The addition ratio of the non-metal catalyst and the epoxide is 1:(50-100) g / g.