Catalyst for preparing olefins from naphtha and its preparation method and application

By designing a catalyst containing HZSM-5 molecular sieve, dehydrogenation metal active components and metal oxides, and regulating the catalytic cracking reaction path, the problem of excessive methane yield in the existing technology was solved, and the naphtha catalysis was achieved. Efficient production of light olefins and suppression of methane generation in cracking.

CN116408137BActive Publication Date: 2024-10-29CHINA UNIV OF PETROLEUM (EAST CHINA) +1
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202310207258.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-07
Publication Date
2024-10-29
Estimated Expiration
2043-03-07

AI Technical Summary

Technical Problem

When the existing naphtha catalytic cracking technology increases the reaction temperature to increase the production of low-carbon olefins, the methane yield is too high, which leads to an increase in separation costs and is difficult to effectively control.

Method used

Design a catalyst, including 20-60% carrier, 20-60% molecular sieve, 0.5-20% metal active component and 10-30% binder, using HZSM-5 molecular sieve and dehydrogenation metal active component Components, auxiliary metal active components and metal oxides are used to regulate the catalytic cracking reaction path, reduce the generation of free radicals and inhibit the generation of methane through the preparation method of modified molecular sieves and carrier slurries.

Benefits of technology

Maintain hydrocarbon conversion rate at lower temperatures, change the type of free radicals, and combine metal dehydrogenation and acidic site reaction capabilities to effectively inhibit methane generation, improve the selectivity of low-carbon olefins, and reduce methane yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004111311140000061
    Figure BDA0004111311140000061
Patent Text Reader

Abstract

The present invention belongs to the field of catalyst technology, and specifically discloses a catalyst for naphtha to olefins. By weight percentage, the catalyst includes 20-60% of a carrier, 20-60% of a molecular sieve, 0.5-20% of a metal active component and 10-30% of a binder, and the metal active component includes a dehydrogenation metal active component, an auxiliary metal active component and a metal oxide. The molecular sieve is a HZSM-5 molecular sieve, the dehydrogenation metal active component is one or more of Zn, Ni, Co and Ga, the auxiliary metal active component is one or more of Fe and Ce, and the metal oxide component is one or more of CaO and MgO. The present invention also discloses a preparation method and application of the above-mentioned catalyst. The catalyst provided by the present invention can effectively inhibit the generation of methane while catalytically cracking naphtha to increase the production of light olefins.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and in particular relates to a catalyst for preparing olefins from naphtha, and a preparation method and application thereof. Background Art

[0002] As a major component of the chemical industry, about 50 million tons of light olefins are used to produce a series of downstream products each year. However, as the main source of light olefins, steam cracking has limitations such as high reaction temperature (800-900℃), high energy consumption (accounting for 40% of petrochemical energy consumption), large CO2 emissions, and uncontrollable product distribution, which makes it difficult to meet the demand. Therefore, catalytic cracking processes based on naphtha, heavy oil, C4~C8 low value-added olefins and other different raw materials have been widely studied and applied. The naphtha catalytic cracking process stands out among these processes because of its advantages such as a wide range of raw material sources and flexible product distribution. The scale effect and cost advantage make it the most attractive and more likely to replace the original process.

[0003] Catalytic cracking is the process of converting petroleum hydrocarbons into light olefins such as ethylene and propylene under the synergistic effect of acidic zeolite catalysts and high temperature. The presence of acidic catalysts and high temperature determine that the catalytic cracking reaction mechanism is a situation where the positive carbon ion mechanism and the free radical mechanism coexist. Under normal circumstances, when the reaction temperature is low, the positive carbon ion mechanism is dominant in the catalytic cracking reaction, the propylene yield is high, and the ethylene yield is low; when the reaction temperature is high, the free radical mechanism is dominant, and the ethylene yield will increase. The dominant reaction mechanism is different for different catalyst types. In low-temperature cracking on acidic zeolite catalysts, the positive carbon ion reaction mechanism will dominate; in high-temperature cracking on Ca-Al series catalysts, the free radical reaction mechanism will dominate; in medium-temperature cracking on zeolite catalysts with dual active centers, the positive carbon ion mechanism and the free radical mechanism play an important role together.

[0004] Although a number of catalytic cracking technologies for olefin production have been industrialized, these technologies all encounter the technical bottleneck of excessive methane yield when further increasing the production of low-carbon olefins by increasing the reaction temperature. For example, the CPP process developed by Sinopec Research Institute of Petroleum, when the production scheme is adjusted from the propylene scheme (reaction temperature 576°C) to the ethylene scheme (reaction temperature 640°C), its dry gas yield after deducting ethylene increased from 7.87% to 16.76%, an increase of more than 1 times. Excessive methane yield will lead to a significant increase in separation costs.

[0005] Therefore, how to design a catalyst for catalytic cracking of naphtha to effectively control methane generation and maximize the production of olefins becomes the key to solving this bottleneck. Summary of the invention

[0006] One of the purposes of the present invention is to provide a catalyst for preparing olefins from naphtha, which effectively solves the problem of excessively high methane yield when the existing naphtha catalytic cracking technology further increases the production of light olefins by increasing the reaction temperature.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0008] A catalyst for preparing olefins from naphtha, comprising, by weight percentage, 20-60% of a carrier, 20-60% of a molecular sieve, 0.5-20% of a metal active component and 10-30% of a binder, wherein the metal active component comprises a dehydrogenation metal active component, an auxiliary metal active component and a metal oxide.

[0009] Furthermore, the catalyst includes 42% of a carrier, 40% of a molecular sieve, 8% of a metal active component and 10% of a binder.

[0010] Furthermore, the molecular sieve is a HZSM-5 molecular sieve, the dehydrogenation metal active component is one or more of Zn, Ni, Co and Ga, the auxiliary metal active component is one or more of Fe and Ce, and the metal oxide component is one or more of CaO and MgO.

[0011] Furthermore, the silicon-aluminum ratio of the HZSM-5 molecular sieve is 25-300.

[0012] Furthermore, the carrier is selected from one or more of kaolin, bentonite and montmorillonite.

[0013] Furthermore, the binder is selected from one or more of silica sol, alumina sol or pseudo-boehmite.

[0014] The second object of the present invention is to provide a method for preparing the above-mentioned catalyst for naphtha to olefins, comprising the following steps:

[0015] S1. Add molecular sieve into water and stir to obtain a uniform slurry;

[0016] S2, adding the soluble metal salt of the dehydrogenation metal active component and the soluble metal salt of the auxiliary metal active component to the slurry obtained in step S1, stirring sufficiently, filtering, washing, drying at a constant temperature, and then calcining to obtain a modified molecular sieve;

[0017] S3, mixing the metal oxide, the carrier, the binder and water, and stirring them to obtain a carrier slurry;

[0018] S4, adding the modified molecular sieve into the carrier slurry for mixing and slurrying, and then spray drying, washing and filtering in sequence, and then drying at a constant temperature and calcining to obtain a catalyst.

[0019] Furthermore, in steps S2 and S4, the drying temperature is 90-150° C., the drying time is 2-12 hours, and the roasting temperature is 500-700° C., the roasting time is 4-12 hours.

[0020] The third object of the present invention is to provide an application of the above catalyst in catalytic cracking of naphtha to increase the production of light olefins while reducing the methane yield.

[0021] The beneficial technical effects of the present invention are:

[0022] On the one hand, the present invention uses basic metal oxides to reduce the activation energy of free radical generation, promotes free radical reactions under the catalysis of basic active sites, maintains the conversion rate of hydrocarbons at a relatively low temperature, and changes the type of initial free radicals; on the other hand, metal components with dehydrogenation activity are introduced into zeolite, and auxiliary metal components are introduced to improve its anti-sintering stability and dispersibility, thereby realizing the combination of metal dehydrogenation ability and acid site cracking ability, and regulating the selectivity of the positive carbon ion reaction path. Thus, while catalytic cracking of naphtha increases the production of light olefins, methane generation can be effectively suppressed. DETAILED DESCRIPTION

[0023] The following exemplary embodiments will provide further detailed description of the catalyst for preparing olefins from naphtha and its preparation method and application involved in the present invention, but the protection scope of the present invention is not limited thereto.

[0024] In one embodiment, the present invention provides a catalyst for preparing olefins from naphtha, wherein the catalyst comprises, by weight percentage, 20-60% of a carrier, 20-60% of a molecular sieve, 0.5-20% of a metal active component and 10-30% of a binder, wherein the metal active component comprises a dehydrogenation metal active component required for molecular sieve modification, an auxiliary metal active component and a metal oxide added during the catalyst molding process.

[0025] In some preferred embodiments, the catalyst includes 42% of a carrier, 40% of a molecular sieve, 8% of a metal active component and 10% of a binder.

[0026] The molecular sieve is a HZSM-5 molecular sieve, and the silicon-aluminum ratio of the HZSM-5 molecular sieve is 25 to 300. The dehydrogenation metal active component is one or more of Zn, Ni, Co and Ga; the auxiliary metal active component is one or more of Fe and Ce; the metal oxide component is one or more of CaO and MgO. The carrier is selected from one or more of kaolin, bentonite and montmorillonite. The binder is selected from one or more of silica sol, aluminum sol or pseudo-boehmite.

[0027] In some preferred embodiments, the silicon-aluminum ratio of the HZSM-5 molecular sieve is 85, the carrier is kaolin, and the binder is pseudo-boehmite.

[0028] In one embodiment, the present invention provides a method for preparing the above-mentioned catalyst for naphtha to olefins, comprising the following steps:

[0029] S1. Add molecular sieve into water and stir to obtain a uniform slurry.

[0030] S2. Add the soluble metal salt of the dehydrogenation metal active component and the soluble metal salt of the auxiliary metal active component to the slurry obtained in step S1, filter and wash after sufficient stirring, dry at a constant temperature of 90-150° C. for 2-12 hours, and then calcine at 500-700° C. for 4-12 hours to obtain a modified molecular sieve.

[0031] S3, mixing the metal oxide, carrier, binder and water, slurrying and stirring evenly to obtain carrier slurry.

[0032] S4, adding the modified molecular sieve into the carrier slurry, mixing and slurrying, then spray drying, washing and filtering in sequence, drying at a constant temperature of 90-150° C. for 2-12 hours, and then calcining at 500-700° C. for 4-12 hours to obtain a catalyst.

[0033] In some preferred embodiments, in steps S2 and S4, the drying temperature is 100-120° C., and the drying time is 3-6 hours. The calcining temperature is 550-650° C., and the calcining time is 6-10 hours.

[0034] The catalyst of the present invention can effectively inhibit the generation of methane while catalyzing the cracking of naphtha to increase the production of light olefins. From the analysis of the reaction mechanism and reaction path, to improve the selectivity of light olefins and control the methane yield at the same time, one is to change the type of initial free radicals generated, thereby regulating the free radical reaction path and inhibiting the path that is conducive to methane generation; the other is to use ZSM-5 molecular sieve to strengthen The characteristics of acidity and low hydrogen transfer activity are taken into account, and appropriate metal modification is performed on it to selectively control the unimolecular catalytic cracking reaction and inhibit the hydrogen transfer reaction to ensure high selectivity for olefins.

[0035] Based on this, the present invention, on the one hand, utilizes alkaline metal oxides to reduce the activation energy of free radical generation, promotes free radical reactions under the catalysis of alkaline active sites, maintains the conversion rate of hydrocarbons at a relatively low temperature, and changes the type of initial free radicals; on the other hand, introduces metal components with dehydrogenation activity into zeolite, and introduces auxiliary metal components to improve its anti-sintering stability and dispersibility, thereby achieving a combination of metal dehydrogenation ability and acidic site cracking ability, and regulating the selectivity of the positive carbon ion reaction path.

[0036] The present invention will now be illustrated by the following non-limiting examples. All reagents used below, unless otherwise specified, are chemically pure reagents.

[0037] The HZSM-5 molecular sieve used was produced by Tianjin Nanhua Catalyst Factory, wherein SiO2 / Al2O3=85, and was calcined at 550°C for 4 hours before use to remove impurities.

[0038] The metal salts are all nitrates.

[0039] The metal oxides were all commercially available.

[0040] Kaolin is an industrial product of Suzhou Kaolin Company.

[0041] Pseudo-boehmite is a product of Shandong Aluminum Plant.

[0042] Example 1

[0043] 50g of HZSM-5 molecular sieve was added to 120g of deionized water and stirred to obtain a slurry. Then, 2.28g of Zn(NO3)2·6H2O and 3.62g of Fe(NO3)3·9H2O were added to the slurry, stirred thoroughly, filtered, washed, and dried at 110°C for 6 hours. Then, the slurry was calcined at 550°C for 6 hours to obtain a modified molecular sieve.

[0044] 3 g of CaO, 45 g of kaolin and 10 g of pseudo-boehmite were added to 90 g of deionized water, slurried and stirred to obtain a carrier slurry.

[0045] 40 g of the modified molecular sieve was added to the carrier slurry for mixing and slurrying, followed by spray drying, washing, filtering, and then drying at 120° C. for 5 hours and calcining at 650° C. for 7 hours to obtain catalyst CAT-1.

[0046] Example 2

[0047] The method of Example 1 is followed, except that 2.48 g Ni(NO3)2·6H2O is used instead of Zn(NO3)2·6H2O in Example 1 to obtain catalyst CAT-2.

[0048] Example 3

[0049] The method of Example 1 was followed, except that 1.55 g of Ce(NO3)3·6H2O was used instead of Fe(NO3)3·9H2O in Example 1 to obtain catalyst CAT-3.

[0050] Example 4

[0051] The method of Example 1 is followed, except that MgO is used instead of CaO in Example 1, to obtain catalyst CAT-4.

[0052] Comparative Example 1

[0053] 50 g of HZSM-5 molecular sieve was added to 120 g of deionized water and stirred to obtain a slurry. Then, 2.28 g of Zn(NO3)2·6H2O was added to the slurry, stirred thoroughly, filtered, washed, and dried at 110°C for 6 hours. Then, the slurry was calcined at 550°C for 6 hours to obtain a modified molecular sieve.

[0054] 3 g of CaO, 45 g of kaolin and 10 g of pseudo-boehmite were added to 90 g of deionized water, slurried and stirred to obtain a carrier slurry.

[0055] 40 g of the modified molecular sieve was added to the carrier slurry for mixing and slurrying, followed by spray drying, washing, filtering, and then drying at 120° C. for 5 hours and calcining at 650° C. for 7 hours to obtain catalyst CAT-D1.

[0056] Comparative Example 2

[0057] 50 g of HZSM-5 molecular sieve was added to 120 g of deionized water and stirred to obtain a slurry. Then, 2.28 g of Zn(NO3)2·6H2O was added to the slurry, stirred thoroughly, filtered, washed, and dried at 110°C for 6 hours. Then, the slurry was calcined at 550°C for 6 hours to obtain a modified molecular sieve.

[0058] Take 45g of kaolin and 10g of pseudo-boehmite, add them into 90g of deionized water, beat and stir to obtain a carrier slurry.

[0059] 40 g of the modified molecular sieve was added to the carrier slurry for mixing and slurrying, followed by spray drying, washing, filtering, and then drying at 120° C. for 5 hours and calcining at 650° C. for 7 hours to obtain catalyst CAT-D2.

[0060] Comparative Example 3

[0061] 50 g of HZSM-5 molecular sieve was added to 120 g of deionized water and stirred to obtain a slurry, which was then filtered, washed, and dried at 110° C. for 6 hours. The slurry was then calcined at 550° C. for 6 hours to obtain molecular sieve I.

[0062] Take 45g of kaolin and 10g of pseudo-boehmite, add them into 90g of deionized water, beat and stir to obtain a carrier slurry.

[0063] 40 g of the molecular sieve I was added to the carrier slurry for mixing and slurrying, followed by spray drying, washing, filtering, and then drying at 120° C. for 5 hours and calcining at 650° C. for 7 hours to obtain catalyst CAT-D3.

[0064] Catalytic cracking of naphtha using the catalysts prepared in Examples 1-4 and Comparative Examples 1-3 respectively comprises the following steps: before the reaction, the catalyst is hydrothermally aged at 700°C for 4 hours with a water injection rate of 2 mL / min. During the reaction, a fixed bed microreactor is used to load 6 g of the catalyst into a reaction tube, and then the reactor is sealed and heated to a reaction temperature of 650°C, and the air in the reaction tube and the impurities adsorbed on the catalyst are replaced with N2; after 2 hours, naphtha is introduced into the reaction tube for reaction at a weight hourly space velocity of 10 h -1 , the agent-oil ratio is 2, the reaction pressure is 0.1MPa, and finally the gas phase and liquid phase products are collected separately, and the product yield is calculated.

[0065] The composition of the naphtha raw material is shown in Table 1, and the yield of the target product after catalytic cracking of naphtha by each catalyst is shown in Table 2.

[0066] Table 1 Naphtha raw material composition

[0067] type Content wt% Alkanes 81.91 Olefins 9.68 Cycloalkanes 8.26 Aromatics 0.15

[0068] Table 2 Distribution of target products after catalytic cracking of naphtha by catalysts prepared in various embodiments and comparative examples

[0069]

[0070] As shown in Table 2, among Examples 1-4, the catalyst CAT-1 of Example 1 has the best catalytic effect, the highest diene yield and the lowest methane yield. The catalytic effects of the catalysts CAT-D1 to CAT-D3 of Comparative Examples 1-3 are all worse than those of the catalysts CAT-1 to CAT-4 of Examples 1-4, and the catalytic effects of the catalysts of Comparative Examples 1-3 are CAT-D1>CAT-D2>CAT-D3.

[0071] In the preparation process of the catalysts of each embodiment, the dehydrogenation metal active component of CAT-1 is Zn, the auxiliary metal active component is Fe, and the metal oxide component is CaO; compared with CAT-1, CAT-2 changes the type of dehydrogenation metal, CAT-3 changes the type of auxiliary metal, and CAT-4 changes the type of metal oxide. This shows that when preparing the catalyst, the dehydrogenation metal active component is preferably Zn, the auxiliary metal active component is preferably Fe, and the metal oxide component is preferably CaO.

[0072] Compared with the examples, no auxiliary metal component was added during the preparation of the catalyst CAT-D1 of comparative example 1; no auxiliary metal component and metal oxide were added during the preparation of the catalyst CAT-D2 of comparative example 2; and the catalyst CAT-D3 of comparative example 3 was only an unmodified molecular sieve, and no various metal components were added during the preparation. This shows that the use of the catalyst provided by the present invention to catalytically crack naphtha to produce light olefins can effectively improve the diene yield while inhibiting methane generation.

Claims

1. A method for preparing a catalyst for naphtha to olefins, characterized in that: The catalyst comprises, by weight percentage, 20-60% of a carrier, 20-60% of a molecular sieve, 0.5-20% of a metal active component and 10-30% of a binder, wherein the metal active component comprises a dehydrogenation metal active component, an auxiliary metal active component and a metal oxide; The molecular sieve is HZSM-5 molecular sieve, the dehydrogenation metal active component is one or more of Zn, Ni, Co and Ga, the auxiliary metal active component is one or more of Fe and Ce, and the metal oxide component is one or more of CaO and MgO; The preparation method comprises the following steps: S1. Add molecular sieve into water and stir to obtain a uniform slurry; S2, adding the soluble metal salt of the dehydrogenation metal active component and the soluble metal salt of the auxiliary metal active component to the slurry obtained in step S1, stirring sufficiently, filtering, washing, drying at a constant temperature, and then calcining to obtain a modified molecular sieve; S3, mixing the metal oxide, the carrier, the binder and water, and stirring them to obtain a carrier slurry; S4, adding the modified molecular sieve into the carrier slurry for mixing and slurrying, and then spray drying, washing and filtering in sequence, and then drying at a constant temperature and calcining to obtain a catalyst.

2. The method for preparing a catalyst for naphtha to olefins according to claim 1, characterized in that: The catalyst comprises 42% of a carrier, 40% of a molecular sieve, 8% of a metal active component and 10% of a binder.

3. The method for preparing a catalyst for naphtha to olefins according to claim 2, characterized in that: The silicon-aluminum ratio of the HZSM-5 molecular sieve is 25-300.

4. The method for preparing a catalyst for naphtha to olefins according to claim 3, characterized in that: The carrier is selected from one or more of kaolin, bentonite and montmorillonite.

5. The method for preparing a catalyst for naphtha to olefins according to claim 4, characterized in that: The binder is selected from one or more of silica sol, alumina sol or pseudo-boehmite.

6. The method for preparing a catalyst for naphtha to olefins according to claim 5, characterized in that: In steps S2 and S4, the drying temperature is 90-150° C., the drying time is 2-12 hours, and the calcining temperature is 500-700° C., the calcining time is 4-12 hours.

7. Use of a catalyst prepared by the method for preparing a catalyst according to any one of claims 1 to 6 in catalytic cracking of naphtha to increase the production of light olefins while reducing the methane yield.

Citation Information

Patent Citations

  • Fluid bed catalyst for producing olefin by catalytic cracking method

    CN101190414A

  • Method of preparing olefin by catalytic cracking

    CN101190862A

  • Method for catalytically converting naphtha into light olefins

    CN102465001A

  • Catalyst used for dehydrogenation preparation of monoolefine by saturated alkane

    CN105289622A

  • Catalyst for catalytic dehydrogenation of alkane as well as preparation method and application method of catalyst

    CN105618026A