Unburned bricks prepared from water-based drilling cuttings and method thereof
By adding glass fiber and optimizing the formula to the preparation of water-based drilling cuttings, the problems of low utilization rate of mud cuttings and insufficient compressive strength have been solved, efficient water-based drilling cuttings resource reuse has been achieved, and no-burning bricks have been ensured. intensity and environmental benefits.
Patent Information
- Application Number
- CN202111675845.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-12-31
AI Technical Summary
When designing the formula of the existing non-burning bricks prepared from water-based drilling cuttings, the added amount of mud cuttings accounts for more than 50% and the utilization rate is low. The compressive strength is insufficient, and spots appear on the surface of the bricks when the cuttings are not crushed, which makes the bricks resistant. The compressive strength is only 3~4MPa, which fails to meet the requirements.
By adding glass fiber and optimizing the formula, the amount of cement and soil binder is small, the tensile and flexural strength of the unfired bricks are improved, the mass ratio of cement and soil binder is controlled within 20%, and the water-based drilling cuttings are crushed to Below 2mm, combined with the use of glass fiber and water-based epoxy resin curing agent, it forms an efficient bonding performance.
It significantly improves the compressive strength and utilization rate of unfired bricks, ensures that the strength and leaching toxicity of the finished product meet standard requirements, reduces costs, avoids powdering, and protects the ecological environment of the oil field.
Smart Images

Figure CN116409964B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of resource utilization of water-based drilling cuttings, and specifically relates to a fired-free brick prepared from water-based drilling cuttings and a method thereof. Background Art
[0002] The exploration and development of oil and gas fields first requires drilling operations. Drilling is the use of oil drilling equipment to drill through multiple formations along the designed track from the ground to reach the predetermined target layer, forming oil and gas wells to achieve the purpose of oil and gas extraction. A large amount of drilling cuttings waste will be generated during the drilling process. At present, water-based drilling cuttings waste has begun to be collected and processed while drilling, but the disposal of water-based drilling cuttings has not been effectively solved, and oil fields are facing the dual pressure of production costs and environmental protection. Oil and gas field exploration and development companies produce a large amount of water-based drilling cuttings each year, which currently need to be outsourced for processing, and the amount and corresponding costs have a trend of continuous increase. However, third-party processing plants lack effective disposal methods and occupy a large amount of land for centralized temporary storage, which poses huge environmental risks. For example, the Changqing Oilfield Branch of China National Petroleum Corporation produces more than 1.5 million cubic meters of water-based drilling cuttings each year, and the current outsourcing processing fee is about 380 million yuan / year.
[0003] The main methods of water-based drilling cuttings resource utilization trials currently being carried out are: paving well site roads and cuttings pressing and molding for reuse. There are mainly the following situations. Daniudi Gas Field uses water-based drilling cuttings instead of sand to pave the road leading to the well station; Southern Petroleum Exploration and Development Co., Ltd. uses solid-phase pressed cakes of waste cuttings generated during the treatment of water-based drilling mud as new building materials; Southwest Oil and Gas Field Company Safety, Environmental Protection and Technical Supervision Research Institute will use the waste cuttings generated by water-based drilling mud to make unburned bricks; Sichuan Qing Drilling East Sichuan Drilling Company will entrust a third party to process waste cuttings generated by water-based drilling mud and use clay and cuttings to mix and make sintered bricks for oilfield infrastructure construction, realizing the recycling of solid waste resources. In addition, according to currently disclosed patents and other information, one type of existing water-based drilling cuttings used to make unburned bricks is to use cement, cuttings, gravel, and sand in a proportion to make unburned bricks, see application number CN200610042967.1, named Chinese patent application of drilling cuttings in unburned brick materials; the other type is to use lime, cement, cuttings, early strength agent (sodium chloride, calcium chloride), water reducer (calcium lignin sulfonate), gel breaker (aluminum salt or iron salt), etc., in a proportion to make unburned bricks. The finished bricks have high compressive and flexural strengths, and all indicators of the leachate meet the secondary standard requirements of GB8978-1996 "Comprehensive Sewage Discharge Standard", see application number CN201711229264.4, named A kind of unburned brick made of waste mud and its preparation method.
[0004] However, the above mud and rock chips have the following problems in making unburned bricks: when designing the formula, the amount of mud and rock chips added accounts for more than 50%, and the utilization rate of mud and rock chips is low (below 50%), which is not economical. The unburned bricks made by the Sichuan Qing Drilling Chuandong Drilling Company mentioned in the previous paragraph using rock chips and commissioned to a third party were severely powdered after one year, and were not very practical; when preparing unburned bricks, the rock chips were not crushed and mixed with curing agent, cement, and rock chips to make bricks. After testing, the commonly used water-based epoxy resin curing agent and cement were selected and mixed in a ratio of 0.3‰:14%. The trial-produced unburned bricks had spots on the surface of the finished unburned bricks and the compressive strength was 3-4MPa. Figure 1 As shown, it does not meet the requirements. The reason is that the rock cuttings contain soil blocks, and the curing agent cannot penetrate and work. Therefore, it is necessary to improve the formula and preparation method of water-based drilling cuttings to prepare unburned bricks. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a method for preparing unfired bricks using water-based drilling cuttings. The tensile and flexural strengths of the unfired bricks are improved by adding glass fiber, and the amount of cement and chemicals added is small. This solves the problem of large amount of cement added and low utilization rate of cuttings when preparing unfired bricks using water-based drilling cuttings, ensures that the strength and leaching toxicity of the unfired bricks meet the standard requirements, and achieves good environmental benefits.
[0006] The present invention is achieved through the following technical solutions:
[0007] The invention discloses an unburned brick prepared from water-based drilling cuttings. The aggregate of the unburned brick comprises the following components by weight: 100 parts of water-based drilling cuttings, 6 to 16 parts of cement, 1 part of glass fiber and 0.014 to 0.026 parts of soil binder.
[0008] Preferably, the cement is No. 32.5 cement or No. 42.5 cement.
[0009] Preferably, the particle size of the water-based drilling cuttings is less than 2 mm.
[0010] Preferably, the soil binder is a water-based epoxy resin curing agent.
[0011] Preferably, the unburned bricks are grass-planted bricks; the cement is 10 to 12 parts, and the soil binder is 0.014 to 0.016 parts.
[0012] Preferably, the unburned bricks are solid square bricks; the cement is 14 to 16 parts, and the soil binder is 0.022 to 0.024 parts.
[0013] Preferably, the unfired brick is a U-shaped trough or a pipeline cover; the cement is 12 to 14 parts, and the soil binder is 0.018 to 0.02 parts.
[0014] A method for preparing any of the above-mentioned unburned bricks from water-based drilling cuttings comprises the following steps:
[0015] The aggregate of any one of the above-mentioned unburned bricks is evenly mixed with water to obtain a mixed liquid, the mixed liquid is pressed into shape, and then cured according to the curing method of concrete bricks to obtain the corresponding unburned bricks.
[0016] Furthermore, the mass ratio of aggregate to water of the unfired brick is 0.3:1.
[0017] Furthermore, the aggregate of the unburned brick and water are stirred at 300-450 rpm for 30-60 seconds.
[0018] Compared with the prior art, the present invention has the following beneficial technical effects:
[0019] The present invention discloses an unburned brick prepared from water-based drilling cuttings. Adding soil binder to water-based drilling cuttings can enhance its bonding performance to improve the compressive strength of unburned bricks. The mixing ratio of cement, glass fiber, soil binder and water-based drilling cuttings in unburned bricks of different shapes and types is finally determined. Adding glass fiber can improve the tensile and flexural strength of unburned bricks. The amount of cement and agent added is small. The mass ratio of cement and soil binder added in aggregate is within 20%, which has obvious advantages over other prior arts with an amount of more than 50%. The present invention has a small amount of cement added, which is less than 20% of the total mass of aggregate, which is lower than the current amount of 50% to 60%, and has lower cost. The amount of water-based drilling cuttings added accounts for more than 50% of the total mass of aggregate, and the utilization rate of water-based drilling cuttings is high.
[0020] Furthermore, the water-based drilling cuttings are crushed to less than 2 mm and used as components to meet the grading requirements of sintered brick raw materials. The mudstone particles in the water-based drilling cuttings will swell and crush when they come into contact with water, which will reduce the compressive strength of the sample. Through experiments, it was determined that pre-treating the water-based drilling cuttings and crushing them to less than 2 mm will have little effect on the compressive strength.
[0021] The present invention discloses a method for preparing unburned bricks from water-based drilling cuttings. The method comprises the following steps: firstly, the aggregate of the unburned bricks is uniformly mixed with water to obtain a mixed liquid, and the mixed liquid is pressed and molded. The finished bricks after pressing and curing meet the strength and leaching toxicity requirements of the standards. The prepared unburned bricks have high consolidation strength, strong consolidation and elimination ability for harmful substances, high erosion and soaking resistance, and will not pulverize after 3 years, thereby protecting the ecological environment of the oil field. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a physical picture of the unfired brick sample prepared when the rock chips are not crushed in the prior art.
[0023] Figure 2 This is a real picture of the solid square brick sample prepared after the rock cuttings are crushed according to the present invention.
[0024] Figure 3 This is a real picture of the grass bricks prepared by crushing rock chips according to the present invention. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solutions and advantages of the present invention more clear, the following further describes the implementation mode of the present invention in detail in conjunction with specific embodiments, which are intended to explain the present invention rather than limit it.
[0026] The present invention discloses an unburned brick prepared from water-based drilling cuttings, which includes a formula of the unburned brick. The unburned bricks are divided into grass-planting bricks, solid square bricks, U-shaped grooves and pipeline covers according to different shapes and types. The unburned bricks of different shapes are described below.
[0027] The formula of the grass brick includes the following components by weight:
[0028] Water-based drilling cuttings: cement: glass fiber: soil binder = 100: (6-16): 1: (0.014-0.026).
[0029] The formula of solid square bricks, in parts by weight, includes the following components:
[0030] Water-based drilling cuttings: cement: glass fiber: soil binder = 100: (10-16): 1: (0.022-0.026).
[0031] The formula of the U-shaped trough and the pipeline cover is the same, and includes the following components by weight:
[0032] Water-based drilling cuttings: cement: glass fiber: soil binder = 100: (6-14): 1: (0.018-0.022).
[0033] The cement mentioned above is No. 32.5 cement or No. 42.5 cement. The soil binder is a water-based epoxy resin curing agent, and the mixture formed by the above formula is called aggregate.
[0034] The present invention provides a method for preparing unburned bricks using water-based drilling cuttings, comprising the following steps:
[0035] Step a. Measuring: According to the above weight ratio, drilling cuttings, cement, soil binder, glass fiber and water are mixed to form a mixed liquid. The weight ratio of water to aggregate is 0.3:1.
[0036] Step b. Stirring: The mixed solution is mechanically stirred, and the stirring speed is generally controlled at 300-450 rpm, and the cycle is generally controlled at 30s-60s.
[0037] Step c. Molding: Select the corresponding mold according to the specifications of the finished product, and use the hydraulic brick machine to press and shape it.
[0038] Step d. Curing: The curing method of the finished drilling cuttings is the same as that of ordinary concrete bricks. Generally, it is required to wait 28 days after the curing is completed before use.
[0039] Embodiment 1:
[0040] Preparation of grass bricks
[0041] The formula is based on water-based drilling cuttings: 32.5 cement: glass fiber: water-based epoxy Resin Curing agent = 100:16:1:0.026. After stirring at 450rpm for 30s, the brick was pressed into shape by a hydraulic brick machine and cured for 28 days. It was normal after soaking in water for 200h. The compressive strength was 10.47Mpa, and no powdering occurred. The prepared finished products met the requirements.
[0042] In addition, when the formula dosage is changed, when the ratio of the amount of waterborne epoxy resin curing agent to the water-based drilling cuttings is 0.018%, the ratio of the amount of cement to the water-based drilling cuttings is 6%. After molding and curing for 28 days, the compressive strength of the finished product prepared after soaking is 5.58Mpa, which is smaller than 10.47Mpa, but meets the requirements of NY / T 1253-2006 "Grass Planting Brick" standard (compressive strength ≧5MPa);
[0043] When the ratio of waterborne epoxy resin curing agent to water-based drilling cuttings is 0.016%, the ratio of cement to water-based drilling cuttings is 8%, and the product is molded and cured for 28 days. The compressive strength of the finished product prepared after soaking is 5.33Mpa, which is smaller than 10.47Mpa, but meets the requirements of NY / T1253-2006 "Grass Brick" standard.
[0044] When the ratio of waterborne epoxy resin curing agent to water-based drilling cuttings is 0.014%, the ratio of cement to water-based drilling cuttings is 10%, and the molding and curing for 28 days, the finished product prepared after soaking has a compressive strength of 5.43Mpa, which is smaller than 10.47Mpa, but meets the requirements of NY / T1253-2006 "Grass Brick" standard.
[0045] Since the price of soil binder water-based epoxy resin curing agent is very high compared with cement, from the perspective of cost saving, the amount of soil binder should be reduced as much as possible. Therefore, the optimized formula is water-based drilling cuttings: cement: glass fiber: soil binder = 100: (10-12): 1: (0.014-0.016).
[0046] Embodiment 2:
[0047] Preparation of grass bricks
[0048] The formula is water-based drilling cuttings: No. 42.5 cement: glass fiber: hydrogenated methylnadic anhydride (H-MNA) = 100:16:1:0.026. The results show that it is normal after soaking in water for 200 hours, and there is no powdering phenomenon after molding and curing for 28 days. The compressive strength is 5.98Mpa. The strength and leaching toxicity of the prepared finished product meet the requirements.
[0049] from Figure 3 It can be seen that the grass bricks obtained in this embodiment have no spots and are compact.
[0050] Embodiment three:
[0051] Preparation of grass bricks
[0052] The formula is water-based drilling cuttings: No. 32.5 cement: glass fiber: T-99 super flexible multifunctional epoxy resin curing agent = 100:16:1:0.026. The results show that it is normal after immersion in water for 200 hours, and there is no powdering phenomenon after molding and curing for 28 days. The compressive strength is 6.82Mpa, and the strength and leaching toxicity of the prepared finished product meet the requirements.
[0053] Comparative Example 1:
[0054] Preparation of grass bricks
[0055] The formula is water-based drilling cuttings: 42.5 cement: glass fiber: Epon HPT curing agent 1061 = 100: 16: 1: 0.026. The results show that it is normal after immersion in water for 200 hours, but powdering occurs after molding and curing for 28 days. The prepared finished product does not meet the requirements.
[0056] Comparative Example 2:
[0057] Preparation of grass bricks
[0058] The formula was water-based drilling cuttings: No. 32.5 cement: glass fiber: Ajicure PN-31 soil binder = 100:16:1:0.026. The results showed that dissolution occurred after immersion in water for 200 hours, and the prepared finished product did not meet the requirements.
[0059] Embodiment 4:
[0060] Preparation of solid square bricks
[0061] When the ratio of water-based epoxy resin curing agent to water-based drilling cuttings is 0.026%, after stirring, the brick is pressed and formed by a hydraulic brick machine, and cured for 28 days, and then soaked in water for 200 hours, the ratio of cement to water-based drilling cuttings is 10%. The compressive strength of the finished product can be greater than 15Mpa, and no powdering occurs. The prepared finished products all meet the requirements of JC / T 422-2007 "Non-sintered garbage tailings bricks" standard (compressive strength ≧15MPa).
[0062] In addition, when the formula dosage is changed, when the ratio of water-based epoxy resin curing agent to water-based drilling cuttings is 0.024%, and the ratio of cement to water-based drilling cuttings is 12%, the compressive strength of the prepared finished product can be greater than 15Mpa, which meets the requirements of JC / T 422-2007 "Non-sintered garbage tailings bricks" standard.
[0063] When the ratio of waterborne epoxy resin curing agent to water-based drilling cuttings is 0.022%, and the ratio of cement to water-based drilling cuttings is 14%, the compressive strength of the finished product can be greater than 15Mpa, which meets the requirements of JC / T 422-2007 "Non-sintered waste tailings bricks" standard.
[0064] From the perspective of cost saving, the amount of soil binder should be minimized, so the optimized solid square brick formula is drilling cuttings: cement: glass fiber: soil solidifier = 100: (14-16): 1: (0.022-0.024).
[0065] from Figure 2 It can be seen that the solid square bricks obtained in this embodiment have no spots and are compact.
[0066] Embodiment five:
[0067] Preparation of U-shaped grooves and pipeline covers
[0068] When the ratio of waterborne epoxy resin curing agent to water-based drilling cuttings is 0.022%, and the ratio of cement to water-based drilling cuttings is 6%, the finished product can meet the requirements of GB50164-2011 "Concrete Quality Control Standard" (compressive strength ≧10MPa).
[0069] In addition, when the formula dosage is changed, when the ratio of waterborne epoxy resin curing agent to water-based drilling cuttings is 0.020%, and the ratio of cement to water-based drilling cuttings is 8%, the finished product meets the requirements of GB50164-2011 "Concrete Quality Control Standard" (compressive strength ≧10MPa);
[0070] When the ratio of waterborne epoxy resin curing agent to water-based drilling cuttings is 0.018%, and the ratio of cement to water-based drilling cuttings is 12%, the finished product meets the requirements of GB50164-2011 "Concrete Quality Control Standard" (compressive strength ≧10MPa).
[0071] From the perspective of cost saving, the amount of soil binder should be minimized, so the optimized U-shaped trough and pipeline cover formula is drilling cuttings: cement: glass fiber: soil solidifier = 100: (12-14): 1: (0.018-0.02).
[0072] The above examples are merely illustrative of the present invention and do not constitute a limitation on the protection scope of the present invention. All designs that are the same or similar to the present invention fall within the protection scope of the present invention.
Claims
1. A method for preparing unburned bricks from water-based drilling cuttings, characterized in that: The water and the aggregate are mixed evenly in a mass ratio of 0.3:1 to obtain a mixed liquid, the mixed liquid is pressed into a shape, and then cured according to the curing method of concrete bricks to obtain the corresponding unburned bricks; Calculated by weight, the aggregate of the unburned bricks includes the following components: 100 parts of water-based drilling cuttings, 6 to 16 parts of cement, 1 part of glass fiber and 0.014 to 0.026 parts of soil binder, the particle size of the water-based drilling cuttings is less than 2 mm, and the soil binder is a water-based epoxy resin curing agent.
2. The method for preparing unburned bricks from water-based drilling cuttings according to claim 1, characterized in that: The cement is No. 32.5 cement or No. 42.5 cement.
3. The method for preparing unburned bricks from water-based drilling cuttings according to claim 1, characterized in that: The unburned bricks are grass-planted bricks; the cement is 10 to 12 parts, and the soil binder is 0.014 to 0.016 parts.
4. The method for preparing unburned bricks from water-based drilling cuttings according to claim 1, characterized in that: The unburned bricks are solid square bricks; the cement is 14 to 16 parts, and the soil binder is 0.022 to 0.024 parts.
5. The method for preparing unburned bricks from water-based drilling cuttings according to claim 1, characterized in that: The unburned brick is a U-shaped groove or a pipeline cover; the cement is 12 to 14 parts, and the soil binder is 0.018 to 0.02 parts.
6. The method for preparing unburned bricks from water-based drilling cuttings according to claim 1, characterized in that: The aggregate of the unburned brick and water are stirred at 300-450 rpm for 30-60 seconds.
Citation Information
Patent Citations
Application of well drilling detritus in baking-free brick material
CN101085702A
A method for preparing non-fired bricks from waste mud.
CN107840623B
Drilling wastes recycling method
CN105347609A