Amorphous alloy material and preparation process thereof

By adjusting the elemental composition of amorphous alloy materials and adding elements such as zirconium and nickel, modified zirconium oxide and aluminum oxide films are formed, which solves the problem of insufficient corrosion resistance of iron-based amorphous alloy materials in harsh environments and achieves high corrosion resistance. Corrosive and environmentally friendly effects.

CN116411228BActive Publication Date: 2024-10-22SHENZHEN TOPSUN TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310529798.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-10-22
Estimated Expiration
2043-05-11

AI Technical Summary

Technical Problem

Iron-based amorphous alloy materials have poor corrosion resistance in harsh environments such as moisture, salt and alkali, and large-scale use of chromium will pollute the environment, making it difficult to meet the demand for high corrosion resistance.

Method used

By adjusting the elemental composition of the amorphous alloy material, including the proportions of iron, chromium, copper, silicon, boron, carbon and titanium, and adding zirconium and nickel elements to the alloy, it is covered with modified zirconium oxide and aluminum oxide films to improve the resistance to corrosion. corrosive.

Benefits of technology

The corrosion resistance of amorphous alloy materials is significantly improved, the annual corrosion rate is reduced to 4.1×10-2mm/a, the Vickers hardness is 635-689, it has high hardness and erosion and wear resistance, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004224184630000071
    Figure BDA0004224184630000071
  • Figure BDA0004224184630000081
    Figure BDA0004224184630000081
Patent Text Reader

Abstract

The present application relates to the technical field of metal materials, and specifically discloses an amorphous alloy material and its preparation process, an amorphous alloy material, which includes the following elements in percentage by weight: 88‑92% iron, 0.08‑0.1% chromium, 0.3‑0.5% copper, 4‑6% silicon, 2‑3% boron, 0.05‑0.1% carbon and 0.4‑0.8% titanium, with the remainder being unavoidable impurities. The Vickers hardness of the amorphous alloy material obtained in the present application is 635‑689, the minimum unit weight loss due to erosion and wear is 3.7 mg / h, and the maximum saturation magnetic induction intensity can reach 1.40T, with high hardness, erosion and wear resistance and magnetic properties. And the annual corrosion rate of the amorphous alloy material obtained in the present application can be as low as 4.1×10 ‑2 mm / a, which improves the corrosion resistance of amorphous alloy materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of metal materials, and more specifically, to an amorphous alloy material and a preparation process thereof. Background Art

[0002] Amorphous alloy materials are metal alloys that retain the disordered atomic structure of the liquid in the solid state by cooling the alloy melt at a high speed so that the atoms in the alloy melt do not have time to arrange in order. Amorphous alloy materials are widely used in military, aerospace, petrochemical and other fields due to their high strength and wear resistance. Iron-based amorphous alloy is a more common type of amorphous alloy material. In actual practical use, its corrosion resistance is poor and it is difficult to meet the needs of use in harsh environments such as humidity, salt and alkali.

[0003] In the related art, in order to improve the corrosion resistance of iron-based amorphous alloy materials, copper and nickel elements are usually added to the raw materials of iron-based amorphous alloy materials, so that copper and nickel elements form a passivation film on the surface of the amorphous alloy materials, but its corrosion resistance is still low. And when chromium elements are added to amorphous alloy materials, the chromium content must be greater than 12% to make the amorphous alloy materials show good corrosion resistance, but the large-scale use of chromium elements will cause pollution to the soil and water sources and cause harm to the environment. Therefore, how to produce amorphous alloy materials with high corrosion resistance to replace traditional metal materials is a major issue in the research of amorphous alloy materials. Summary of the invention

[0004] In order to improve the corrosion resistance of amorphous alloys, the present application provides an amorphous alloy material and a preparation process thereof.

[0005] In a first aspect, the present application provides an amorphous alloy material, which adopts the following technical solution:

[0006] An amorphous alloy material comprises the following elements in percentage by weight: 88-92% iron, 0.08-0.1% chromium, 0.3-0.5% copper, 4-6% silicon, 2-3% boron, 0.05-0.1% carbon and 0.4-0.8% titanium, with the remainder being inevitable impurities.

[0007] The amorphous alloy material elements of the present application can be selected from 90-92% iron, 0.08-0.1% chromium, 0.3-0.5% copper, 4-5% silicon, 2-3% boron, 0.05-0.1% carbon and 0.4-0.8% titanium. Any value within the respective ranges can be selected, and the corrosion resistance of the amorphous alloy material can be improved. The best effect is achieved when the iron content is 91%, the chromium content is 0.09%, the copper content is 0.4%, the silicon content is 5.43%, the boron content is 2%, the carbon content is 0.08% and the titanium content is 0.6%.

[0008] By adopting the above technical scheme, with iron as the basic element, it has high saturation magnetic induction intensity, high hardness and high corrosion resistance. Chromium can make up for the deficiency of Cr in the chromium-poor zone caused by voids and oxidation defects in the alloy during the corrosion process, and improve the corrosion resistance of amorphous alloy materials. Copper can increase the disorder of the amorphous alloy system, thereby changing the amorphous forming ability of the amorphous alloy. The addition of silicon is beneficial to improving the thermal stability, corrosion resistance and stability of the passivation film of the amorphous alloy. Boron can improve the hardness and thermal stability of the amorphous alloy material. Carbon can effectively enhance the corrosion resistance of metal materials. Titanium can promote the formation of amorphous alloys and improve the corrosion resistance of amorphous alloy materials.

[0009] Preferably, the amorphous alloy material further comprises the following elements in percentage by weight: zirconium 0.4-0.8%.

[0010] The amorphous alloy material elements of the present application can be selected from 90-92% iron, 0.08-0.1% chromium, 0.3-0.5% copper, 4-5% silicon, 2-3% boron, 0.05-0.1% carbon, 0.4-0.8% zirconium and 0.4-0.8% titanium. Any value within the respective ranges can be selected, and the corrosion resistance of the amorphous alloy material can be improved. The best effect is achieved when the iron content is 90.57%, the chromium content is 0.09%, the copper content is 0.4%, the silicon content is 5.52%, the boron content is 2%, the carbon content is 0.08%, the zirconium content is 0.44% and the titanium content is 0.6%.

[0011] By adopting the above technical solution, the addition of zirconium enhances the interatomic interaction in the amorphous alloy, which can significantly reduce the crystallization temperature range during the solidification process, and improve the amorphous forming ability and compression fracture strength of the alloy. Moreover, zirconium and boron can synergistically promote the formation of amorphous alloys.

[0012] Preferably, the weight percentage of zirconium to boron is 1:(3-6).

[0013] By adopting the above technical solution and adjusting the weight percentage ratio of zirconium to boron, the corrosion resistance of the amorphous alloy material can be further improved.

[0014] Preferably, the zirconium is derived from zirconium oxide, and the zirconium oxide is modified by oxalic acid to obtain modified zirconium oxide.

[0015] By adopting the above technical solution, zirconium oxide is treated with oxalic acid to improve its surface properties, so that it has better surface stability, forms high-strength and high-density physical and chemical properties, and improves the corrosion resistance of the amorphous alloy material.

[0016] Preferably, the modified zirconium oxide is prepared by the following steps:

[0017] 1-3 kg of oxalic acid and 19-25 kg of toluene are added to 60-70 L of water, and zirconium oxide and silane coupling agent are added, dispersed evenly, calcined at 1500-1600° C. for 3-6 hours, cooled, and crushed to obtain modified zirconium oxide.

[0018] By adopting the above technical scheme, zirconium oxide powder is added to a solution of water and a saturated toluene solution containing adipic acid, and the zirconium oxide is treated with adipic acid to improve its surface properties and give it better surface stability. It is then treated with a silane coupling agent to form high-strength and high-density physical and chemical properties, thereby improving corrosion resistance and significantly reducing the occurrence of cracks.

[0019] Preferably, the amorphous alloy material further comprises raw materials in the following weight percentages: 1-2% aluminum and 0.5-1% nickel.

[0020] By adopting the above technical solution, aluminum reacts with oxygen in the air to form a dense aluminum oxide film covering the surface of the amorphous alloy material. On the one hand, nickel can improve the combination of aluminum and other elements and improve the wettability of the interface between the matrix. On the other hand, both nickel and aluminum can improve the corrosion resistance of the amorphous alloy material.

[0021] Preferably, the weight percentage of nickel to aluminum is 1:(2-3).

[0022] By adopting the above technical solution and adjusting the weight percentage of nickel and aluminum, the corrosion resistance of the amorphous alloy material can be further improved.

[0023] In a second aspect, the present application provides a preparation process of an amorphous alloy material, which is specifically achieved through the following technical solutions:

[0024] An amorphous alloy material, comprising the following steps:

[0025] The raw materials of the amorphous alloy material are vacuum smelted, heated and melted, uniformly added to a steel ingot mold, cooled to obtain an alloy ingot, re-smelted at 1340-1360° C., poured onto a copper roller, cooled to obtain an amorphous alloy material.

[0026] By adopting the above technical scheme, the raw materials of the amorphous alloy material are vacuum smelted, heated and melted, and uniformly added to the steel ingot mold, cooled to obtain the alloy ingot. The uniform speed of adding to the steel ingot mold can reduce the internal pores of the alloy ingot and improve the strength of the amorphous alloy material; the alloy ingot is then secondary smelted at 1340-1360℃, injected onto the copper roller, and cooled to obtain the amorphous alloy material.

[0027] Preferably, each element is cleaned with alcohol before vacuum smelting, heating and melting.

[0028] By adopting the above technical solution, each element is cleaned with alcohol before vacuum smelting, heating and melting, so as to remove impurities on the surface of the material and improve the bonding strength between the elements, thereby improving the corrosion resistance of the amorphous alloy material.

[0029] In summary, the present application includes at least one of the following beneficial technical effects:

[0030] (1) This application controls the elements in the amorphous alloy material and the proportion of each element to make the annual corrosion rate of the amorphous alloy material 5.1×10 -2 mm / a, which improves the corrosion resistance of amorphous alloy materials.

[0031] (2) The present invention adds zirconium to the amorphous alloy material and controls the weight percentage of zirconium and boron to make the annual corrosion rate of the amorphous alloy material 4.8×10 -2 ~4.9×10 -2 mm / a, further improving the corrosion resistance of amorphous alloy materials.

[0032] (3) In the present invention, by adjusting the amount of oxalic acid in the process of modifying zirconium oxide, the annual corrosion rate of the amorphous alloy material is 4.4×10 -2 ~4.6×10 -2 mm / a, further improving the corrosion resistance of amorphous alloy materials.

[0033] (4) The present invention adds nickel and aluminum elements to the amorphous alloy material and adjusts the percentage ratio of the two elements to make the annual corrosion rate of the amorphous alloy material 4.1×10 -2 ~4.2×10 -2 mm / a, further improving the corrosion resistance of amorphous alloy materials.

[0034] (5) The Vickers hardness of the amorphous alloy material obtained in this application is 635-689, the minimum unit weight loss due to erosion and wear is 3.7 mg / h, and the maximum saturation magnetic induction intensity can reach 1.40 T. It has high hardness, erosion and wear resistance, and magnetic properties. The annual corrosion rate of the amorphous alloy material obtained in this application can be as low as 4.1×10 -2 mm / a, which improves the corrosion resistance of amorphous alloy materials. DETAILED DESCRIPTION

[0035] The present application is further described in detail below in conjunction with specific embodiments.

[0036] The following elements in this application are all commercially available products, and are intended to make the elements of this application fully disclosed, and should not be understood as limiting the sources of the elements. Specifically: iron, derived from ferroferric oxide; chromium, derived from chromium carbide; copper, derived from copper oxide; silicon, derived from silicon dioxide; boron, derived from boron oxide; carbon, derived from zirconium carbide; titanium, derived from titanium dioxide; silane coupling agent, KH550 is selected; aluminum, derived from aluminum oxide; nickel, derived from nickel oxide.

[0037] The following is an example of the preparation of modified zirconium oxide

[0038] Preparation Example 1

[0039] The modified zirconium oxide of Preparation Example 1 is prepared by the following steps:

[0040] 0.5 kg of oxalic acid and 23 kg of toluene were added to 65 L of water and mixed, and 1 kg of zirconium oxide and 30 g of silane coupling agent were added, dispersed evenly, calcined at 1500° C. for 5 h, cooled, and crushed to a particle size of 0.1 mm to obtain modified zirconium oxide.

[0041] Preparation Example 2

[0042] The modified zirconium oxide of Preparation Example 2 is prepared by the following steps:

[0043] 1 kg of oxalic acid and 23 kg of toluene were added to 65 L of water and mixed, and 1 kg of zirconium oxide and 30 g of silane coupling agent were added, dispersed evenly, calcined at 1500° C. for 5 h, cooled, and crushed to a particle size of 0.1 mm to obtain modified zirconium oxide.

[0044] Preparation Example 3

[0045] The modified zirconium oxide of Preparation Example 3 is prepared by the following steps:

[0046] 2 kg of oxalic acid and 23 kg of toluene were added to 65 L of water and mixed, and 1 kg of zirconium oxide and 30 g of silane coupling agent were added, dispersed evenly, calcined at 1500° C. for 5 h, cooled, and crushed to a particle size of 0.1 mm to obtain modified zirconium oxide.

[0047] Preparation Example 4

[0048] The modified zirconium oxide of Preparation Example 4 is prepared by the following steps:

[0049] 3 kg of oxalic acid and 23 kg of toluene were added to 65 L of water and mixed, and 1 kg of zirconium oxide and 30 g of silane coupling agent were added, dispersed evenly, calcined at 1500° C. for 5 h, cooled, and crushed to a particle size of 0.1 mm to obtain modified zirconium oxide.

[0050] Preparation Example 5

[0051] The modified zirconium oxide of Preparation Example 5 is prepared by the following steps:

[0052] 3.5 kg of oxalic acid and 23 kg of toluene were added to 65 L of water and mixed, and 1 kg of zirconium oxide and 30 g of silane coupling agent were added, dispersed evenly, calcined at 1500° C. for 5 h, cooled, and crushed to a particle size of 0.1 mm to obtain modified zirconium oxide.

[0053] Example 1

[0054] An amorphous alloy material is prepared by the following steps:

[0055] According to the dosage in Table 1, ferroferric oxide, chromium carbide, copper oxide, silicon dioxide, boron oxide and titanium dioxide are mixed and melted in vacuum, added to a steel ingot mold at a uniform speed, cooled to obtain an alloy ingot, and re-smelted at 1350°C, injected onto a copper roller, and cooled to obtain an amorphous alloy material.

[0056] Example 2-3

[0057] The amorphous alloy materials of Examples 2-3 are completely the same in preparation method and element types as those of Example 1, except that the doping amounts of each element are different, as shown in Table 1 for details.

[0058] Table 1 Proportion of each element in the amorphous alloy material of Examples 1-3 (unit: %)

[0059] element Example 1 Example 2 Example 3 iron 91 91 91 chromium 0.08 0.09 0.1 copper 0.4 0.4 0.4 silicon 5.54 5.43 5.52 boron 2 2 2 carbon 0.08 0.08 0.08 titanium 0.6 0.6 0.6 Unavoidable impurities 0.3 0.4 0.3

[0060] Embodiment 4-8

[0061] The amorphous alloy materials of Examples 4-8 are prepared in the same manner as that of Example 2, except that the amorphous alloy materials further include zirconium elements, wherein the zirconium elements are derived from zirconium oxide. The specific doping amount is shown in Table 2.

[0062] Table 2 Proportion of each element in the amorphous alloy materials of Examples 4-8 (unit: %)

[0063] element Example 4 Example 5 Example 6 Example 7 Example 8 iron 90.01 90.24 90.57 90.68 89.58 chromium 0.09 0.09 0.09 0.09 0.09 copper 0.4 0.4 0.4 0.4 0.4 silicon 5.52 5.52 5.52 5.52 5.52 boron 2 2 2 2 3 zirconium 1 0.67 0.44 0.33 0.43 carbon 0.08 0.08 0.08 0.08 0.08 titanium 0.6 0.6 0.6 0.6 0.6 Unavoidable impurities 0.3 0.4 0.3 0.3 0.3

[0064] Examples 9-13

[0065] The preparation method of the amorphous alloy materials of Examples 9-13 is the same as that of Example 6, except that the zirconium element in the amorphous alloy materials comes from the modified zirconium oxide prepared in Preparation Examples 1-5, and the types and doping amounts of other elements are the same as those of Example 6.

[0066] Examples 14-18

[0067] The amorphous alloy materials of Examples 14-18 are prepared in the same manner as that of Example 11, except that the amorphous alloy materials further include aluminum and nickel elements, and the specific doping amounts are shown in Table 3.

[0068] Table 3 Proportion of each element in the amorphous alloy materials of Examples 14-18 (unit: %)

[0069] element Embodiment 14 Embodiment 15 Example 16 Embodiment 17 Embodiment 18 iron 89 89.5 89.25 89 88.5 chromium 0.09 0.09 0.09 0.09 0.09 copper 0.4 0.4 0.4 0.4 0.4 silicon 5.52 5.52 5.52 5.52 5.52 boron 2 2 2 2 2 zirconium 0.44 0.44 0.44 0.44 0.44 carbon 0.08 0.08 0.08 0.08 0.08 titanium 0.6 0.6 0.6 0.6 0.6 aluminum 1 1 1.25 1.5 2 nickel 1 0.5 0.5 0.5 0.5 Unavoidable impurities 0.3 0.4 0.3 0.3 0.3

[0070] Comparative Example 1

[0071] The preparation method of the amorphous alloy material of Comparative Example 1 is exactly the same as that of Example 1, except that the chromium element in the amorphous alloy material is replaced by an equal amount of iron element, and the remaining elements and doping amounts are the same as those of Example 1.

[0072] Comparative Example 2

[0073] The preparation method of the amorphous alloy material of Comparative Example 2 is exactly the same as that of Example 1, except that the silicon element in the amorphous alloy material is replaced by an equal amount of iron element, and the remaining elements and doping amounts are the same as those of Example 1.

[0074] Comparative Example 3

[0075] The preparation method of the amorphous alloy material of Comparative Example 3 is exactly the same as that of Example 1, except that the boron element in the amorphous alloy material is replaced by an equal amount of iron element, and the remaining elements and doping amounts are the same as those of Example 1.

[0076] Comparative Example 4

[0077] The preparation method of the amorphous alloy material of Comparative Example 4 is exactly the same as that of Example 1, except that the titanium element in the amorphous alloy material is replaced by an equal amount of iron element, and the remaining elements and doping amounts are the same as those of Example 1.

[0078] Performance Testing

[0079] The following testing standards or methods were used to test the performance of the amorphous alloy materials obtained in different Examples 1-18 and Comparative Examples 1-4. The test results are shown in Table 4.

[0080] Vickers hardness: According to GB / T 7997-2014 "Test method for Vickers hardness of cemented carbide", HV5 is selected to test the Vickers hardness of amorphous alloy materials.

[0081] Unit weight loss due to erosion and wear: 50-mesh quartz sand was selected as the erosion particles and sprayed onto the test surface at an erosion speed of 10 m / s under normal temperature and pressure conditions. The concentration of the erosion particles in the slurry was 8%, the erosion angle was 45 degrees, and the unit weight loss due to erosion and wear was finally tested.

[0082] Annual corrosion rate: The annual corrosion rate of amorphous alloy materials is calculated according to JB / T 7901-1999 “Laboratory uniform corrosion full immersion test for metal materials”, where the corrosion is a neutral sodium chloride solution with a mass concentration of 3.5wt%.

[0083] Saturation magnetic induction intensity: Use a vibrating sample magnetometer to detect the saturation magnetic induction intensity of amorphous alloy materials.

[0084] Table 4 Performance test results of different amorphous alloy materials

[0085]

[0086]

[0087] The test results in Table 4 show that the Vickers hardness of the amorphous alloy material obtained in this application is 635-689, the minimum unit weight loss due to erosion and wear is 3.7 mg / h, and the maximum saturation magnetic induction intensity can reach 1.40 T, which has high hardness, erosion and wear resistance and magnetic properties. The annual corrosion rate of the amorphous alloy material obtained in this application can be as low as 4.1×10 -2 mm / a, which improves the corrosion resistance of amorphous alloy materials.

[0088] In Examples 1-3, the annual corrosion rate of the amorphous alloy material in Example 2 is 5.1×10 -2 mm / a, which are lower than those in Example 1 and Example 3, indicating that the proportions of the elements in the amorphous alloy material in Example 2 are more appropriate, which improves the corrosion resistance of the amorphous alloy material. This may be related to the fact that the elements can make up for the lack of Cr in the chromium-depleted area caused by voids and oxidation defects in the alloy during the corrosion process, thereby improving the corrosion resistance of the amorphous alloy material.

[0089] In Examples 4-8, the annual corrosion rate of the amorphous alloy material in Example 5-7 is 4.8×10 -2 ~4.9×10 -2 mm / a, which are lower than those in Example 4 and Example 8, indicating that the weight percentage of zirconium to boron in the amorphous alloy material is 1:(3-6) which is more suitable, and improves the corrosion resistance of the amorphous alloy material. This may be related to the fact that zirconium and boron can synergistically promote the formation of amorphous alloys, and adjusting the weight percentage ratio of zirconium to boron can further improve the corrosion resistance of amorphous alloy materials.

[0090] In Examples 9-13, the annual corrosion rate of the amorphous alloy material in Examples 10-12 is 4.4×10 -2 ~4.6×10 - 2mm / a, which are lower than those in Example 9 and Example 13, indicating that the amount of oxalic acid in Examples 10-12 is more appropriate when modifying zirconium oxide, and the corrosion resistance of the amorphous alloy material is improved. This may be related to the fact that adjusting the amount of oxalic acid can improve the effect of oxalic acid treatment of zirconium oxide, thereby further improving the corrosion resistance of the amorphous alloy material.

[0091] In Examples 14-18, the annual corrosion rate of the amorphous alloy material in Examples 15-17 is 4.1×10 -2 ~4.2×10 -2 mm / a, which are lower than those in Example 14 and Example 18, indicating that the weight percentage of nickel to aluminum in the amorphous alloy material is 1:(2-3) which is more suitable, and the corrosion resistance of the amorphous alloy material is improved. This may be related to the fact that nickel can improve the combination of aluminum and other elements and improve the wettability of the interface between the substrates, and that both nickel and aluminum can improve the corrosion resistance of the amorphous alloy material.

[0092] In summary, when the amorphous alloy material includes the following weight percentage elements: 88-92% iron, 0.08-0.1% chromium, 0.3-0.5% copper, 4-6% silicon, 2-3% boron, 0.05-0.1% carbon and 0.4-0.8% titanium, and the balance is inevitable impurities, the amorphous alloy material has higher hardness, erosion and wear resistance and magnetic properties, and improves the corrosion resistance of the amorphous alloy material. The amorphous alloy material can also add zirconium elements, and by adjusting the weight percentage of zirconium and boron elements and controlling them at 1: (3-6), the corrosion resistance of the amorphous alloy material can be further improved.

[0093] Secondly, zirconium oxide, the source of zirconium element, is modified and treated with oxalic acid to improve its surface properties, so that it has better surface stability, forms high-strength and high-density physical and chemical properties, and improves the corrosion resistance of the amorphous alloy material. The effect of oxalic acid treatment of zirconium oxide is improved by further controlling the dosage of oxalic acid, thereby further improving the corrosion resistance of the amorphous alloy material.

[0094] Finally, the present application adds aluminum and nickel elements to the amorphous alloy material, so that aluminum reacts with oxygen in the air to generate a dense aluminum oxide film covering the surface of the amorphous alloy material. The nickel element improves the combination of aluminum and other elements and improves the wettability of the interface between the matrix, thereby improving the corrosion resistance of the amorphous alloy material. And by adjusting the weight percentage of nickel and aluminum and controlling it at 1: (2-3), the corrosion resistance of the amorphous alloy material is further improved.

[0095] Combining the performance test data of the amorphous alloy materials of Comparative Examples 1-4 and Example 1, it is found that adding chromium, silicon, boron and titanium elements to the amorphous alloy material can improve the corrosion resistance of the amorphous alloy material to varying degrees.

[0096] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An amorphous alloy material, characterized in that: It includes the following elements in percentage by weight: 88-92% iron, 0.08-0.1% chromium, 0.3-0.5% copper, 4-6% silicon, 2-3% boron, 0.05-0.1% carbon, 0.4-0.8% titanium, 0.4-1% zirconium, and the remainder is unavoidable impurities; the weight percentage of zirconium to boron is 1:(3-6); The zirconium is derived from zirconium oxide, and the zirconium oxide is modified by oxalic acid to obtain modified zirconium oxide; The modified zirconium oxide is prepared by the following steps: 1-3 kg oxalic acid and 19-25 kg toluene are added to 60-70 L water for mixing, 1-2 kg zirconium oxide and 20-50 g silane coupling agent are added, dispersed evenly, calcined at 1500-1600° C. for 4-6 hours, cooled, and crushed to obtain the modified zirconium oxide.

2. The amorphous alloy material according to claim 1, characterized in that: The amorphous alloy material also includes raw materials with the following weight percentages: 1-2% aluminum and 0.5-1% nickel.

3. The amorphous alloy material according to claim 2, characterized in that: The weight percentage of nickel to aluminum is 1:(2-3).

4. A process for preparing the amorphous alloy material according to any one of claims 1 to 3, characterized in that: The steps include: The raw materials of the amorphous alloy material are vacuum smelted, heated and melted, uniformly added to a steel ingot mold, cooled to obtain an alloy ingot, re-smelted at 1340-1360° C., poured onto a copper roller, cooled to obtain an amorphous alloy material.

5. The process for preparing the amorphous alloy material according to claim 4, characterized in that: The above-mentioned elements are cleaned with alcohol before vacuum smelting, heating and melting.