A method for moisturizing dam concrete core sample

By coating the water-based moisturizing material and covering the saturated interlayer on the surface of the dam concrete core sample, combined with the multi-layer composite structure of the flexible insulation material, the water loss problem of the core sample in dry and cold environments is solved, and the test results are improved accuracy and authenticity of concrete properties.

CN116413103BActive Publication Date: 2024-11-01CHINA THREE GORGES CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310185101.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-01
Publication Date
2024-11-01
Estimated Expiration
2043-03-01

AI Technical Summary

Technical Problem

After removal, the dam concrete core sample is prone to water loss or frost damage due to dry and cold conditions, resulting in large differences in the performance test results from the actual performance, and the existing moisturizing methods have limited effects.

Method used

The core sample surface is coated with water-based moisturizing material, coated with a saturated sandwich material, and sealed with flexible insulation materials, and constructed a multi-layer composite structure to lock water, increase moisture and protect moisture, and fill with flexible compressible materials to prevent damage.

Benefits of technology

It achieves long-term and effective moisturizing under different environmental conditions, improves the accuracy of core sample test results, reflects the true characteristics of concrete, and reduces the risk of damage during transportation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004103450690000051
    Figure BDA0004103450690000051
  • Figure BDA0004103450690000061
    Figure BDA0004103450690000061
  • Figure BDA0004103450690000081
    Figure BDA0004103450690000081
Patent Text Reader

Abstract

A method for moisturizing a dam concrete core sample belongs to the technical field of core sample moisturizing, overcomes the defect of poor moisturizing effect on dam concrete core samples in the prior art, and improves the accuracy of concrete core sample test results. The method for moisturizing a dam concrete core sample of the present invention comprises the following steps: step 1, coating a water-based moisturizing material on the surface of the core sample after the core sample is taken out; step 2, coating an interlayer on the surface of the core sample, wherein the interlayer material is in a saturated state; step 3, sealing the core sample with a flexible thermal insulation material. The present invention can achieve a long-lasting and effective moisturizing effect, and the moisturizing method is simple and easy to implement with low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of core sample moisturizing, and in particular relates to a moisturizing method for a dam concrete core sample. Background Art

[0002] In order to check the pouring quality of dam concrete or understand its true performance, core samples of dam concrete are often drilled, and a comprehensive evaluation is conducted after observing its apparent quality, testing its comprehensive properties such as mechanics, deformation, and durability.

[0003] Most dam concrete is three-grade or four-grade concrete with a maximum aggregate size of 80mm or 150mm. In order to truly reflect the distribution of dam concrete aggregates, the core diameter is generally not less than 150mm. In order to fully understand the performance of dam concrete, there are many core sample testing items. Under the premise of minimizing the impact of drilling on the dam structure, the length of the dam concrete core sample is generally greater than 1m. The humidity of the concrete inside the dam is high and it is in a constant humidity state for a long time. Due to the difference between the service environment of the dam concrete core sample inside the dam body and the natural environment, if the core sample is not immediately moisturized after drilling, it is easy to cause the core sample to dry out and lose water during placement or transportation, or be frozen and damaged in cold weather conditions. There is a big difference between the performance test results and the actual performance of the dam concrete.

[0004] At present, there is no standard process and method for moisturizing concrete core samples. After drilling concrete core samples at the construction site, they are generally not processed and are placed directly in the core sample box; a few are simply wrapped with plastic film for moisturizing; and some are placed in a pool or painted with a layer of varnish on the surface after coring for display purposes. When wrapped with plastic film for moisturizing, the surface humidity of the concrete core sample is easily affected by the external environment and reduced, especially since it takes a long time for the core sample to be drilled out from the dam body and transported to the laboratory, and the moisturizing effect of the core sample is limited. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present invention is to overcome the defect of poor moisturizing effect on dam concrete core samples in the prior art and provide a moisturizing method for dam concrete core samples.

[0006] To this end, the present invention provides the following technical solutions.

[0007] A method for moisturizing a dam concrete core sample comprises the following steps:

[0008] Step 1: After the core sample is taken out, a water-based moisturizing material is applied on the surface of the core sample;

[0009] Step 2, coating the surface of the core sample with an interlayer, wherein the interlayer material is in a saturated water state;

[0010] Step 3: Use flexible thermal insulation material to seal the core sample.

[0011] Furthermore, in step 1, the aqueous moisturizing material is at least one of fatty alcohol, fatty acid or fatty amine.

[0012] Furthermore, the coating thickness of the aqueous moisturizing material is 0.05 mm to 0.10 mm.

[0013] Furthermore, the interlayer thickness is 1.0 cm to 3.0 cm.

[0014] Furthermore, the interlayer material is at least one of sponge and fiber cotton.

[0015] Furthermore, the flexible thermal insulation material is an aluminum foil rubber-plastic thermal insulation material or a hydrophobic glass wool roll felt, and the flexible thermal insulation material is water-impermeable.

[0016] Furthermore, the thickness of the flexible thermal insulation material is 1.0 cm to 3.0 cm.

[0017] Furthermore, the method also includes step 4, placing the sealed core samples in a sealed container, and filling the gaps between the core samples with flexible compressible materials.

[0018] Furthermore, the flexible compressible material is foam, rubber or wood chips.

[0019] Furthermore, in step 1, after the core sample is taken out, the surface of the core sample is first rinsed and wiped with a towel to make the surface of the core sample moisturized, and then the water-based moisturizing material is applied.

[0020] The water-based moisturizing material is an amphiphilic compound that inhibits water evaporation by forming an insoluble liquid molecular film on the surface of the core sample; the interlayer material is a porous material with strong water absorption and water storage capabilities, which enhances the wetness of the core sample surface; the flexible thermal insulation material maintains the humidity of the interlayer material through thermal insulation measures, and at the same time avoids frost damage to the core sample with a moist surface due to the influence of ambient temperature under cold climate conditions.

[0021] The technical solution of the present invention has the following advantages:

[0022] 1. The method for moisturizing a dam concrete core sample provided by the present invention comprises the following steps: step 1, coating a water-based moisturizing material on the surface of the core sample after the core sample is taken out; step 2, coating an interlayer on the surface of the core sample, wherein the interlayer material is in a saturated state; step 3, sealing the surface of the core sample with a flexible thermal insulation material.

[0023] The present invention uses a technical method of coating a water-based moisturizing material on the surface of the core sample to lock in water, a saturated interlayer material to humidify, and a water-impermeable thermal insulation material to protect moisture, to construct a multi-layer composite structure, and through the synergistic effect between the multi-layer materials, ensure that the core sample can achieve a long-term and effective moisturizing effect under different environmental conditions such as dry heat and cold. The core sample test results are affected by surface water loss during long-distance transportation, and the accuracy of the core sample test results can be improved to reflect the true characteristics of the dam concrete. The moisturizing method of the present invention is simple, easy to operate, and low-cost.

[0024] 2. The method for moisturizing the dam concrete core sample provided by the present invention further includes placing the sealed core sample in a sealed container and filling the gaps between the core samples with a flexible compressible material. This can prevent the core sample from being broken or damaged due to impact during transportation, and avoid the loss of the core sample and the impact on its performance detection.

[0025] 3. In step 1 of the present invention, after the core sample is taken out, the surface of the sample is first rinsed and wiped with a towel to make the surface of the core sample moist, and then the water-based moisturizing material is applied. The water-based moisturizing material is characterized by a water-soluble group at one end, which has a hydrophilic property, and a long-chain non-polar group at the other end, which has a hydrophobic property. Its amphiphilic property allows the water-based moisturizing material to spontaneously spread on the moist surface of the core sample to form an insoluble liquid molecular film, thereby inhibiting the evaporation of water on the surface of the core sample. DETAILED DESCRIPTION

[0026] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0027] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be purchased commercially.

[0028] Example 1

[0029] The concrete core of a dam gallery was sampled. The concrete design strength index is C 90 30, the designed antifreeze grade is F200.

[0030] This embodiment provides a method for moisturizing a dam concrete core sample, comprising the following steps:

[0031] Step 1: After the core sample is taken out, the surface of the specimen is first rinsed and wiped with a towel to make the surface of the core sample moist, and then coated with a 0.05 mm thick aqueous moisturizing material, which is a compound of hexadecanol and n-propanol in a mass ratio of 0.5:1.0.

[0032] Step 2: Wrap the core sample tightly with a saturated sponge with a thickness of 1.0 cm.

[0033] Step 3: Seal the core sample with aluminum foil rubber insulation material, the thickness of the aluminum foil rubber insulation material is 2.0 cm.

[0034] Step 4: Place the sealed core samples in a wooden box, fill the spaces between the core samples with sawdust, and transport them to the laboratory.

[0035] It took 10 days from drilling the dam concrete core sample out of the dam body to transporting it to the laboratory.

[0036] Comparative Example 1

[0037] The core sample of this comparative example was taken from the same dam as that of Example 1, with the same sampling time and size. The core sample of this comparative example did not include steps 1-3, and the core sample was not subjected to moisture protection. The core sample was directly placed in a natural environment without surface treatment. The core sample of this comparative example was transported under the same conditions as the core sample of Example 1.

[0038] After the core samples arrived at the laboratory, they had reached the design age. According to SL / T 352-2020 "Test Procedure for Hydraulic Concrete", the compressive strength and frost resistance of the core samples of Example 1 and Comparative Example 1 were tested, and the test results are shown in Table 1.

[0039] Table 1 Dam concrete core sample performance test results

[0040]

[0041] It can be seen from Table 1 that the compressive strength of the core samples of Example 1 and Comparative Example 1 both meet the design requirements, but the compressive strength of the core sample of Example 1 is higher than that of the core sample of Comparative Example 1; the antifreeze performance of the core sample of Example 1 meets the design requirements, and the antifreeze performance is significantly higher than that of the core sample of Comparative Example 1; the antifreeze grade of the core sample of Comparative Example 1 is only F75, which is far from meeting the design requirements.

[0042] Example 2

[0043] Core sampling was carried out on the downstream surface of a dam body. The concrete design strength grade was C 90 20, the designed anti-seepage grade is W4, and the designed anti-freeze grade is F100.

[0044] This embodiment provides a method for moisturizing a dam concrete core sample, comprising the following steps:

[0045] Step 1: After the core sample is taken out, the surface of the specimen is first rinsed and wiped with a towel to make the surface of the core sample moist, and then coated with a 0.08 mm thick aqueous moisturizing material, which is a compound of eicosanol and n-pentanol in a mass ratio of 0.35:1.0.

[0046] Step 2: Wrap the core sample tightly with water-saturated fiber cotton. The thickness of the fiber cotton is 2.0 cm.

[0047] Step 3: Seal the core sample with hydrophobic glass wool felt. The thickness of the hydrophobic glass wool felt insulation material is 3.0 cm.

[0048] Step 4: Place the sealed core samples in a wooden box, fill the spaces between the core samples with foam, and transport them to the laboratory.

[0049] It took seven days from drilling the dam concrete core sample out of the dam body to transporting it to the laboratory.

[0050] Comparative Example 2

[0051] The core sample of this comparative example was taken from the same dam as that of Example 2, with the same sampling time and size. The core sample of this comparative example did not include steps 1-3, and the core sample was not subjected to moisture protection. The core sample was directly placed in a natural environment without surface treatment. The core sample of this comparative example was transported under the same conditions as the core sample of Example 2.

[0052] When the core samples arrived at the laboratory, they had not reached the design age. The core sample protective materials were removed, and the core samples of Example 2 and Comparative Example 2 were placed under standard curing conditions and cured to the design age. According to SL / T 352-2020 "Test Procedure for Hydraulic Concrete", the core samples were tested for their impermeability and frost resistance. The test results are shown in Table 2.

[0053] Table 2 Dam concrete core sample performance test results

[0054]

[0055] It can be seen from Table 2 that the compressive strength and anti-seepage performance of Example 2 and the unprotected core sample meet the design requirements, but the water seepage height of the core sample of Example 2 is significantly smaller than that of the core sample of Comparative Example 2. The antifreeze performance of the core sample of Example 2 meets the design requirements, and the antifreeze grade of the core sample of Comparative Example 2 is F50, which does not meet the design requirements.

[0056] Comparative Example 3

[0057] The core sample of this comparative example was taken from the same dam as Example 1, with the same sampling time and size. The difference is that the core sample of this comparative example only uses plastic film for moisture retention protection.

[0058] Comparative Example 4

[0059] This comparative example is substantially the same as Example 1, except that this comparative example does not include step 1.

[0060] Comparative Example 5

[0061] This comparative example is substantially the same as Example 1, except that this comparative example does not include step 2.

[0062] Comparative Example 6

[0063] This comparative example is substantially the same as Example 1, except that this comparative example does not include step 3.

[0064] The test results of Comparative Examples 3-6 are shown in Table 3. It can be seen from Table 3 that the concrete core samples adopt the traditional moisturizing method of wrapping with plastic film, that is, the compressive strength and antifreeze performance of the core sample of Comparative Example 3 are lower than those of the core sample of Example 1, especially the antifreeze grade is only F100, which is far from meeting the design requirements. The concrete core samples adopt a double-layer moisturizing structure. Compared with Example 1, they lack water-based moisturizing material (Comparative Example 4), saturated sponge interlayer moisturizing material (Comparative Example 5), and aluminum foil rubber insulation material (Comparative Example 6). The compressive strength and antifreeze performance of the core samples of Comparative Examples 4 to Comparative Examples 6 are slightly lower than those of Example 1, and their antifreeze grades are all F150.

[0065] The above test results show that the protective effect of the double-layer moisturizing structure on the concrete core sample is better than the traditional moisturizing method, but inferior to the multi-layer composite structure proposed in the present invention, which includes water-based moisturizing materials to lock water, saturated interlayer materials to increase humidity, and thermal insulation materials to protect moisture. The synergistic effect between multi-layer materials can achieve a long-lasting and effective moisturizing effect.

[0066] Table 3 Comparison of compressive strength and frost resistance of dam concrete core samples

[0067]

[0068] Obviously, the above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the protection scope of the invention.

Claims

1. A method for moisturizing a dam concrete core sample, characterized in that: The following steps are involved: Step 1: After the core sample is taken out, a water-based moisturizing material is applied on the surface of the core sample; Step 2, coating the surface of the core sample with an interlayer, wherein the interlayer material is in a saturated water state; Step 3, using a flexible thermal insulation material to seal the core sample; In the step 1, the coating thickness of the aqueous moisturizing material is 0.05 mm to 0.10 mm; The aqueous moisturizing material is at least one of fatty alcohol, fatty acid or fatty amine; The material of the interlayer is a porous material, and the thickness of the interlayer is 1.0 cm to 3.0 cm; The flexible thermal insulation material is an aluminum foil rubber-plastic thermal insulation material or a hydrophobic glass wool felt, and the flexible thermal insulation material is water-impermeable; the thickness of the flexible thermal insulation material is 1.0 cm to 3.0 cm; In step 1, after the core sample is taken out, the surface of the core sample is first rinsed and wiped with a towel to make the surface of the core sample moisturized, and then the water-based moisturizing material is applied.

2. The method for moisturizing a dam concrete core sample according to claim 1, characterized in that: The interlayer material is at least one of sponge and fiber cotton.

3. The method for moisturizing a dam concrete core sample according to claim 1 or 2, characterized in that: The method also includes step 4, placing the sealed core samples in a sealed container, and filling the spaces between the core samples with flexible compressible materials.

4. The method for moisturizing a dam concrete core sample according to claim 3, characterized in that: The flexible compressible material is foam, rubber or wood chips.

Citation Information

Patent Citations

  • Concrete moisturizing curing and surface strengthening method

    CN110273553A

  • Cement soil core sample maintenance device

    CN115452499A

  • Coating film curing and reinforcing agent for mortar or concrete

    JP2008285367A