A water-resistant catalyst and its preparation method and application

By using a composite oxide support and palladium-supported method in the catalyst, the problem of performance decay of palladium-based catalysts under water vapor conditions was solved, and efficient low-concentration methane oxidation was achieved, and the methane conversion rate of the catalyst reached more than 80% under aqueous conditions was achieved. .

CN116422324BActive Publication Date: 2024-11-01UNIV OF SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310407803.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-11-01
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

The existing palladium-based catalysts are susceptible to toxicity under water vapor conditions, resulting in a low methane conversion rate and cannot effectively treat low-middle and low concentrations of methane in coal mines.

Method used

The composite oxide support is used to include rod-shaped titanium dioxide and cerium oxide, and is supported by precious metal palladium to activate water molecules through interfacial electron hybridization, alleviate the toxicity of water molecules on active species, and improve the water resistance of the catalyst.

Benefits of technology

The methane conversion rate is significantly improved under aqueous conditions. The methane conversion rate can be as high as 80% when catalyzed with low concentration methane oxidation, and there is almost no attenuation compared to the dry environment. It is suitable for a wide range of methane oxidation applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116422324B_ABST
    Figure CN116422324B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of catalysts, and specifically relates to a water-resistant catalyst and a preparation method and application thereof. The water-resistant catalyst comprises a composite oxide carrier and an active component loaded on the composite oxide carrier, the composite oxide carrier comprises rod-shaped titanium dioxide and cerium oxide, and the active component is a precious metal. The catalyst provided by the present invention can effectively alleviate the poisoning effect of water molecules in the reaction atmosphere on the active substance, significantly improve the water resistance of the catalyst, and when catalyzing the oxidation of low-concentration methane under water-containing conditions, the methane conversion rate can be as high as 80% or more at 400°C, which is almost no attenuation compared to a dry environment, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalysts, and in particular relates to a water-resistant catalyst and a preparation method and application thereof. Background Art

[0002] The coal mine ventilation air generated during coal mining contains low concentrations of methane. Considering that coal mine ventilation air is usually directly discharged into the atmosphere and methane has a strong greenhouse effect, this process is bound to be accompanied by environmental pollution and energy waste. With the development of science and technology, catalytic oxidation technology has become a feasible route for treating low-concentration methane, and has made a series of progress under the promotion of many scientific researchers. The core of catalytic oxidation technology lies in the development of catalyst materials, and palladium-based catalysts have become the most mainstream methane oxidation catalyst materials due to their excellent activation ability for methane molecules. However, the water vapor present in the mine will poison the palladium-based catalyst and significantly reduce its performance, ultimately leading to a low methane conversion rate. Summary of the invention

[0003] The first object of the present invention is to provide a water-resistant catalyst having excellent activity and water resistance for catalyzing low-concentration methane oxidation, aiming to solve the defect that the existing palladium-based catalyst is easily affected by water vapor, resulting in a low methane conversion rate when used for catalytic methane oxidation under water vapor conditions.

[0004] The second object of the present invention is to provide a method for preparing the above-mentioned water-resistant catalyst.

[0005] The third object of the present invention is to provide application of the water-resistant catalyst.

[0006] After in-depth and extensive research, the inventors of the present invention found that the main mechanism of water vapor poisoning palladium-based catalysts is to generate inert palladium hydroxide by adsorption on the surface of active species, and the special crystal faces exposed by rod-shaped titanium dioxide can be interfacially electronically hybridized with cerium oxide, so that water molecules can be activated or adsorbed, so that the poisoning effect of water molecules in the reaction atmosphere on active species can be alleviated, effectively reducing the poisoning of water vapor on the catalyst, improving the water resistance of the catalyst, and thus significantly improving the methane conversion rate. Based on this, the present invention was completed.

[0007] Specifically, the water-resistant catalyst provided by the present invention comprises a composite oxide carrier and an active component loaded on the composite oxide carrier, wherein the composite oxide carrier comprises rod-shaped titanium dioxide and cerium oxide, and the active component is a noble metal.

[0008] The preparation method of the water-resistant catalyst provided by the present invention comprises the following steps:

[0009] S1, dispersing a cerium precursor and rod-shaped titanium dioxide in a solvent, then adding a precipitant to the obtained dispersion and stirring evenly to obtain a mixed solution;

[0010] S2, heating the mixed solution and performing a reflux reaction, cooling the mixed solution to room temperature after the reflux reaction is completed, separating the obtained reaction solution into solid and liquid, and drying and calcining the solid product to obtain a composite oxide support;

[0011] S3, dispersing the composite oxide carrier and the active component precursor in a solvent, evaporating the solvent in the obtained dispersion and then calcining to obtain the water-resistant catalyst.

[0012] In addition, the present invention also provides application of the water-resistant catalyst in a low-concentration methane oxidation process.

[0013] The catalyst provided by the present invention can effectively alleviate the poisoning effect of water molecules in the reaction atmosphere on the active substance, has excellent activity and water resistance in the process of catalyzing low-concentration methane oxidation, and when catalyzing low-concentration methane oxidation under water conditions, the methane conversion rate can be as high as 80% or more at 400°C, which is almost no attenuation compared to a dry environment, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 A is a SEM picture of the rod-shaped titanium dioxide used in Example 1; B is a SEM picture of the water-resistant catalyst obtained in Example 1;

[0015] Figure 2 is the Ce 3d XPS spectrum of the water-resistant catalyst obtained in Example 1;

[0016] Figure 3 The data diagram of the activity and hydrothermal stability of the water-resistant catalyst obtained in Example 1 for catalyzing low-concentration methane oxidation;

[0017] Figure 4 The data diagram of the activity and hydrothermal stability of the water-resistant catalyst obtained in Comparative Example 1 for catalyzing low-concentration methane oxidation;

[0018] Figure 5 This is a data chart of the activity and hydrothermal stability of the water-resistant catalyst obtained in Comparative Example 2 in catalyzing low-concentration methane oxidation. DETAILED DESCRIPTION

[0019] The water-resistant catalyst provided by the present invention comprises a composite oxide carrier and an active component supported on the composite oxide carrier. The composite oxide carrier comprises rod-shaped titanium dioxide and cerium oxide. The active component is a noble metal. The noble metal is particularly preferably palladium.

[0020] In a preferred embodiment of the present invention, based on the total weight of the water-resistant catalyst, the content of the rod-shaped titanium dioxide is 75-98%, the content of the cerium oxide is 1-20%, and the content of the active component is 0.5-5%. At this time, the rod-shaped titanium dioxide, cerium oxide and precious metals can better play a synergistic role, which is more conducive to further improving the methane conversion rate under water-containing conditions. The content of the rod-shaped titanium dioxide is preferably 75-98%, such as 75%, 78%, 80%, 82%, 85%, 88%, 90%, 92%, 95%, 98% or any value therebetween. The content of the cerium oxide is preferably 1-20%, such as 1%, 2%, 4%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20% or any value therebetween; the content of the active component is preferably 0.5-5%, such as 0.5%, 1%, 2%, 3%, 4%, 5% or any value therebetween.

[0021] In the present invention, the aspect ratio of the rod-shaped titanium dioxide is preferably (4-12):1, such as 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1 or any value therebetween.

[0022] In the present invention, the average particle size of the cerium oxide is preferably 5-25 nm, such as 5 nm, 8 nm, 10 nm, 12 nm, 15 nm, 18 nm, 20 nm, 22 nm, 25 nm or any value therebetween.

[0023] In the present invention, the Ce in the water-resistant catalyst 3+ The content of Ce is preferably 25-35wt% of the total cerium content, such as 25wt%, 28wt%, 30wt%, 32wt%, 35wt% or any value therebetween. 3+ When the content of is controlled within the preferred range, the poisoning effect of water molecules in the reaction atmosphere on the active substance can be more effectively alleviated, and the methane conversion rate is better.

[0024] The preparation method of the water-resistant catalyst provided by the present invention comprises the following steps:

[0025] S1, dispersing a cerium precursor and rod-shaped titanium dioxide in a solvent, then adding a precipitant to the obtained dispersion and stirring evenly to obtain a mixed solution;

[0026] S2, heating the mixed solution and performing a reflux reaction, cooling the mixed solution to room temperature after the reflux reaction is completed, separating the obtained reaction solution into solid and liquid, and drying and calcining the solid product to obtain a composite oxide support;

[0027] S3, dispersing the composite oxide carrier and the active component precursor in a solvent, evaporating the solvent in the obtained dispersion and then calcining to obtain the water-resistant catalyst.

[0028] In step S1, the cerium precursor can be various existing compounds that can be converted into cerium oxide, and its specific examples include but are not limited to at least one of cerium nitrate, cerium chloride and cerium sulfate. The precipitation agent can be various existing substances that can precipitate cerium precursor and rod-shaped titanium dioxide, preferably urea and / or hexamethylenetetramine, more preferably a compound of urea and hexamethylenetetramine, which is more conducive to the uniform precipitation of cerium precursor and rod-shaped titanium dioxide, and the activity and water resistance of the obtained catalyst are more excellent, and the methane conversion rate is higher. When the precipitation agent is a compound of urea and hexamethylenetetramine, the mass ratio of urea and hexamethylenetetramine is preferably (0.5-1.5): 1, such as 0.5: 1, 0.7: 1, 0.9: 1, 1: 1, 1.1: 1, 1.3: 1, 1.5: 1 or any value therebetween. The solvent is particularly preferably a mixed solution of ethanol and water, wherein the volume ratio of ethanol to water can generally be (0.5-2):1, such as 0.5:1, 0.8:1, 1:1, 1.2:1, 1.5:1, 1.8:1, 2:1 or any value therebetween. In addition, the rod-shaped titanium dioxide can be used in the form of rod-shaped rutile, for example.

[0029] In step S2, the conditions for the reflux reaction preferably include a temperature of 70-100°C, such as 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C or any value therebetween; a time of 2-10h, such as 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h or any value therebetween. The conditions for the drying preferably include a temperature of 100-130°C, such as 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C or any value therebetween; a time of 3-12h, such as 3h, 5h, 8h, 10h, 12h or any value therebetween. The calcination conditions preferably include a temperature of 300-900°C, such as 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C or any value therebetween; and a time of 3-6h, such as 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h or any value therebetween.

[0030] In step S3, the active component precursor can be any existing compound that can be converted into an active component, preferably a palladium precursor. Specific examples of the palladium precursor include, but are not limited to, at least one of palladium nitrate, palladium chloride and palladium sulfate. The calcination conditions preferably include a temperature of 300-900°C, such as 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C or any value therebetween; the time is 3-6h, such as 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h or any value therebetween. The method of dispersing the composite oxide carrier and the active component precursor in the solvent can be, for example, dispersing the composite oxide carrier and the active component precursor in the solvent respectively, or first dissolving the active component precursor in the solvent to obtain an active component solution, and then placing the obtained composite oxide carrier in the active component solution and stirring evenly. The solvent is preferably water.

[0031] In addition, the present invention also provides application of the water-resistant catalyst in a low-concentration methane oxidation process.

[0032] The water-resistant catalyst provided by the present invention is suitable for the oxidation of methane in a dry environment and is also suitable for the oxidation of methane in a water-containing environment. In addition, the water-resistant catalyst provided by the present invention is suitable for the oxidation of raw materials with high methane concentrations and is also suitable for the oxidation of raw materials with low methane concentrations, and the methane concentration can be as low as 1 vol%.

[0033] The present invention will be described in detail below through examples.

[0034] Example 1

[0035] S1. Take 309.8 mg of Ce(NO3)3·6H2O and 1.0 g of rod-shaped rutile (the aspect ratio is about 10:1, the same below) and add them to 80 mL of a mixed solution of ethanol and water (the volume ratio of ethanol to water is 1:1), add 0.5 g of urea and 0.6 g of hexamethylenetetramine, stir evenly, and obtain a mixed solution;

[0036] S2, transferring the obtained mixed solution to a flask, heating it to 75°C and refluxing it for 4 hours, cooling it to room temperature after the reflux is completed, centrifuging the obtained reaction solution and collecting the solid product, drying it at 100°C for 12 hours, and then calcining it in a muffle furnace at 500°C for 4 hours to obtain a composite oxide carrier;

[0037] S3. Place 0.5 g of the above-mentioned composite oxide carrier in 25.1 mL of palladium nitrate aqueous solution (1 mg / mL) and stir for 3 hours, then heat to evaporate the solvent, and then place it in a muffle furnace and calcine at 500°C for 4 hours to obtain a water-resistant catalyst Pd / TiO2-Ce with a cerium content of 10 wt% and a palladium loading of 2 wt%.

[0038] See also Figure 1 , Figure 1 A is a SEM picture of the rod-shaped rutile used in Example 1, which has an obvious rod-shaped structure and a smooth surface without particles; Figure 1 B is a SEM image of the water-resistant catalyst obtained in Example 1, wherein the rod-shaped material is the titanium dioxide material in A, and the granular material is cerium oxide, and its average particle size is 14 nm. In addition, palladium oxide is a nanoparticle with a smaller particle size, so it is not visible in the SEM image.

[0039] See also Figure 2 , Figure 2 The Ce 3dXPS spectrum of the water-resistant catalyst obtained in Example 1. After fitting the XPS data, it was found that the Ce in the water-resistant catalyst (Pd / TiO2-Ce) 3+ The content of the species is as high as 28.6%; the corresponding Pd-based catalyst supported on commercial cerium oxide (Pd / CeO2) has Ce 3+ The species content is only 13.0%.

[0040] Example 2

[0041] The water-resistant catalyst was prepared according to the method of Example 1, the loading amount of the active component was kept unchanged, and the content of the cerium precursor was adjusted. The specific steps were as follows:

[0042] S1. Take 62.0 mg Ce(NO3)3·6H2O and 1.0 g rod-shaped rutile and add them to 80 mL of a mixed solution of ethanol and water (the volume ratio of ethanol to water is 1:1), add 0.5 g urea and 0.6 g hexamethylenetetramine, stir evenly, and obtain a mixed solution;

[0043] S2, transferring the obtained mixed solution to a flask, heating it to 75°C for reflux reaction for 4 hours, cooling it to room temperature after the reflux is completed, centrifuging the obtained reaction solution and collecting the solid product, drying it at 100°C for 12 hours, and then calcining it in a muffle furnace at 500°C for 4 hours to obtain a composite oxide carrier;

[0044] S3, 0.5g of the composite oxide carrier is placed in 25.1mL of palladium nitrate aqueous solution (1mg / mL) and stirred for 3h, then heated to evaporate the solvent, and then placed in a muffle furnace and calcined at 500°C for 4h to obtain a water-resistant catalyst Pd / TiO2-Ce with a cerium content of 2wt% and a palladium loading of 2wt%, which includes a composite oxide carrier and an active component loaded on the composite oxide carrier, the composite oxide carrier includes rod-shaped titanium dioxide and cerium oxide, and the active component is palladium. The average particle size of cerium oxide in the water-resistant catalyst is 6nm, Ce 3+ The content of cerium accounts for 31.2% of the total cerium content.

[0045] Example 3

[0046] The water-resistant catalyst was prepared according to the method of Example 1, the loading amount of the active component was kept unchanged, and the content of the cerium precursor was adjusted. The specific steps were as follows:

[0047] S1. Take 154.9 mg Ce(NO3)3·6H2O and 1.0 g rod-shaped rutile and add them to 80 mL of a mixed solution of ethanol and water (the volume ratio of ethanol to water is 1:1), add 0.5 g urea and 0.6 g hexamethylenetetramine, stir evenly, and obtain a mixed solution;

[0048] S2, transferring the obtained mixed solution to a flask, heating it to 75°C for reflux reaction for 4 hours, cooling it to room temperature after the reflux is completed, centrifuging the obtained reaction solution and collecting the solid product, drying it at 100°C for 12 hours, and then calcining it in a muffle furnace at 500°C for 4 hours to obtain a composite oxide carrier;

[0049] S3, 0.5g of the composite oxide carrier is placed in 25.1mL of palladium nitrate aqueous solution (1mg / mL) and stirred for 3h, then heated to evaporate the solvent, and then placed in a muffle furnace and calcined at 500°C for 4h to obtain a water-resistant catalyst Pd / TiO2-Ce with a cerium content of 5wt% and a palladium loading of 2wt%, which includes a composite oxide carrier and an active component loaded on the composite oxide carrier, the composite oxide carrier includes rod-shaped titanium dioxide and cerium oxide, and the active component is palladium. The average particle size of cerium oxide in the water-resistant catalyst is 9nm, Ce 3+ The content of cerium accounts for 29.7% of the total cerium content.

[0050] Example 4

[0051] The water-resistant catalyst was prepared according to the method of Example 1, the loading amount of the active component was kept unchanged, and the content of the cerium precursor was adjusted. The specific steps were as follows:

[0052] S1. Take 619.6 mg Ce(NO3)3·6H2O and 1.0 g rod-shaped rutile and add them to 80 mL of a mixed solution of ethanol and water (the volume ratio of ethanol to water is 1:1), add 0.5 g urea and 0.6 g hexamethylenetetramine, stir evenly, and obtain a mixed solution;

[0053] S2, transferring the obtained mixed solution to a flask, heating it to 75°C for reflux reaction for 4 hours, cooling it to room temperature after the reflux is completed, centrifuging the obtained reaction solution and collecting the solid product, drying it at 100°C for 12 hours, and then calcining it in a muffle furnace at 500°C for 4 hours to obtain a composite oxide carrier;

[0054] S3, 0.5g of the composite oxide carrier is placed in 25.1mL of palladium nitrate aqueous solution (1mg / mL) and stirred for 3h, then heated to evaporate the solvent, and then placed in a muffle furnace and calcined at 500°C for 4h to obtain a water-resistant catalyst Pd / TiO2-Ce with a cerium content of 20wt% and a palladium loading of 2wt%, which includes a composite oxide carrier and an active component loaded on the composite oxide carrier, the composite oxide carrier includes rod-shaped titanium dioxide and cerium oxide, and the active component is palladium. The average particle size of cerium oxide in the water-resistant catalyst is 22nm, Ce 3+ The content of cerium accounts for 25.3% of the total cerium content.

[0055] Example 5

[0056] The water-resistant catalyst was prepared according to the method of Example 1, the ratio of titanium dioxide to cerium oxide was kept unchanged, and the content of palladium precursor was adjusted. The specific steps were as follows:

[0057] S1. Take 309.8 mg Ce(NO3)3·6H2O and 1.0 g rod-shaped rutile and add them to 80 mL of a mixed solution of ethanol and water (the volume ratio of ethanol to water is 1:1), add 0.5 g urea and 0.6 g hexamethylenetetramine, stir evenly, and obtain a mixed solution;

[0058] S2, transferring the obtained mixed solution to a flask, heating it to 75°C for reflux reaction for 4 hours, cooling it to room temperature after the reflux is completed, centrifuging the obtained reaction solution and collecting the solid product, drying it at 100°C for 12 hours, and then calcining it in a muffle furnace at 500°C for 4 hours to obtain a composite oxide carrier;

[0059] S3, 0.5g of the composite oxide carrier is placed in 12.05mL of palladium nitrate aqueous solution (1mg / mL) and stirred for 3h, then heated to evaporate the solvent, and then placed in a muffle furnace and calcined at 500°C for 4h to obtain a water-resistant catalyst Pd / TiO2-Ce with a cerium content of 10wt% and a palladium loading of 1wt%, which includes a composite oxide carrier and an active component loaded on the composite oxide carrier, the composite oxide carrier includes rod-shaped titanium dioxide and cerium oxide, and the active component is palladium. The average particle size of cerium oxide in the water-resistant catalyst is 14nm, Ce 3+ The content of cerium accounts for 28.6% of the total cerium content.

[0060] Example 6

[0061] The water-resistant catalyst was prepared according to the method of Example 1, the ratio of titanium dioxide to cerium oxide was kept unchanged, and the content of palladium precursor was adjusted. The specific steps were as follows:

[0062] S1. Take 309.8 mg Ce(NO3)3·6H2O and 1.0 g rod-shaped rutile and add them to 80 mL of a mixed solution of ethanol and water (the volume ratio of ethanol to water is 1:1), add 0.5 g urea and 0.6 g hexamethylenetetramine, stir evenly, and obtain a mixed solution;

[0063] S2, transferring the obtained mixed solution to a flask, heating it to 75°C for reflux reaction for 4 hours, cooling it to room temperature after the reflux is completed, centrifuging the obtained reaction solution and collecting the solid product, drying it at 100°C for 12 hours, and then calcining it in a muffle furnace at 500°C for 4 hours to obtain a composite oxide carrier;

[0064] S3, 0.5g of the composite oxide carrier is placed in 50.2mL of palladium nitrate aqueous solution (1mg / mL) and stirred for 3h, then heated to evaporate the solvent, and then placed in a muffle furnace and calcined at 500°C for 4h to obtain a water-resistant catalyst Pd / TiO2-Ce with a cerium content of 10wt% and a palladium loading of 4wt%, which includes a composite oxide carrier and an active component loaded on the composite oxide carrier, the composite oxide carrier includes rod-shaped titanium dioxide and cerium oxide, and the active component is palladium. The average particle size of cerium oxide in the water-resistant catalyst is 14nm, Ce 3+ The content of cerium accounts for 28.6% of the total cerium content.

[0065] Comparative Example 1

[0066] 0.5 g of rod-shaped rutile material was directly placed in 25.1 mL of palladium nitrate aqueous solution (1 mg / mL) and stirred for 3 h, then heated to evaporate the solvent, and then placed in a muffle furnace and calcined at 500 ° C for 4 h to obtain a palladium-based catalyst (Pd / TiO2) supported on the rod-shaped rutile material.

[0067] Comparative Example 2

[0068] 0.5 g of commercial cerium oxide material was directly placed in 25.1 mL of palladium nitrate aqueous solution (1 mg / mL) and stirred for 3 h, then heated to evaporate the solvent, and then placed in a muffle furnace and calcined at 500 ° C for 4 h to obtain a palladium-based catalyst (Pd / CeO2) supported on the cerium dioxide material.

[0069] Test Case

[0070] The activity evaluation of the catalyst was carried out in a fixed bed tubular microreactor (with an inner diameter of 3 mm), with a catalyst loading of 20 mg, a reaction gas of 1 vol% methane and air, a gas flow rate of 20 mL / min, and a corresponding gas flow space velocity of 60,000 mL / (h·g). After cooling to room temperature, the temperature in the reactor was gradually increased at a rate of 3°C / min. During the temperature increase, the reactor was kept at several selected temperature points for 15 min to allow the reaction to reach a stable state. The methane in the product gas was analyzed online by a GC2100 gas chromatograph equipped with a TCD detector, and the reaction activity was expressed by the conversion rate of methane.

[0071] The evaluation of the water resistance of the catalyst is also based on the above experimental device. A certain flow of deionized water is heated and vaporized through the vaporization chamber (temperature is 140°C) at the front end of the reactor, and the flow of deionized water is controlled by a micro-injection pump.

[0072] See also Figure 3 , Figure 3 The data graph of the activity and hydrothermal stability of the catalyst material obtained in Example 1 for catalytic oxidation of low-concentration methane is shown, wherein the solid line is the performance curve of catalytic oxidation of methane in a dry atmosphere, and the dotted line is the performance curve of catalytic oxidation of methane in an atmosphere containing 8 vol% water vapor. Figure 3 It can be seen that the performance of the catalyst material is attenuated to a certain extent in a water-containing atmosphere, but the degree of performance attenuation in the high temperature range is very low.

[0073] See also Figure 4 , Figure 4 The data graph of the activity and hydrothermal stability of the catalyst material obtained in Comparative Example 1 for catalytic oxidation of low-concentration methane is shown, wherein the solid line is the performance curve for catalytic oxidation of methane in a dry atmosphere, and the dotted line is the performance curve for catalytic oxidation of methane in an atmosphere containing 8 vol% water vapor. Figure 4 It can be seen that the performance of the catalyst material is greatly attenuated in a water-containing atmosphere.

[0074] See also Figure 5 , Figure 5The data graph of the activity and hydrothermal stability of the catalyst material obtained in Comparative Example 2 for catalytic oxidation of low-concentration methane is shown, wherein the solid line is the performance curve for catalytic oxidation of methane in a dry atmosphere, and the dotted line is the performance curve for catalytic oxidation of methane in an atmosphere containing 8 vol% water vapor. Figure 5 It can be seen that the performance attenuation of the catalyst material in a water-containing atmosphere is greater than that of Example 1.

[0075] The conversion rates of methane oxidation catalyzed by the catalysts obtained in the above examples and comparative examples when dried at 400°C and in an atmosphere containing 8 vol% water vapor are shown in Table 1.

[0076] Table 1

[0077]

[0078] As can be seen from the results of Table 1, when the catalyst provided by the present invention catalyzes the oxidation of low-concentration methane under water-containing conditions, the methane conversion rate can be as high as 80% or more at 400°C, which is almost attenuated compared to a dry environment. From the comparison of Example 1 and Comparative Example 1, it can be seen that the performance of the palladium-based catalyst (Pd / TiO2) supported on rod-shaped titanium dioxide in a dry atmosphere is comparable to that of the palladium-based catalyst (Pd / TiO2-Ce) supported on a composite metal oxide, but under water-containing conditions, the performance of Pd / TiO2 is greatly attenuated, and the methane conversion rate at 400°C is only 2.0%, while the methane conversion rate of Pd / TiO2-Ce under the same conditions is as high as 99.3%, which is almost attenuated compared to a dry environment. From the comparison between Example 1 and Comparative Examples 1 and 2, it can be seen that although the attenuation degree of the palladium catalyst (Pd / CeO2) supported on the pure cerium dioxide carrier in Comparative Example 2 after the introduction of water vapor is slightly lower than that of the palladium-based catalyst (Pd / TiO2) supported on the rod-shaped titanium dioxide in Comparative Example 1, the methane conversion rate is still significantly reduced compared with the palladium-based catalyst (Pd / TiO2-Ce) supported on the composite metal oxide in Example 1, indicating that when pure rod-shaped titanium dioxide and cerium dioxide are used as carriers, the water resistance of the palladium catalysts supported thereon is poor.

[0079] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.

Claims

1. A water-resistant catalyst, characterized in that: The water-resistant catalyst includes a composite oxide carrier and an active component loaded on the composite oxide carrier, the composite oxide carrier includes rod-shaped titanium dioxide and cerium oxide, the active component is a precious metal, and based on the total weight of the water-resistant catalyst, the content of the rod-shaped titanium dioxide is 75-98%, the content of the cerium oxide is 1-20%, and the content of the active component is 0.5-5%.

2. The water-resistant catalyst according to claim 1, characterized in that The aspect ratio of the rod-shaped titanium dioxide is (4-12):1; and the average particle size of the cerium oxide is 5-25 nm.

3. The water-resistant catalyst according to claim 1 or 2, characterized in that: The Ce in the water-resistant catalyst 3+ The content of cerium accounts for 25-35wt% of the total cerium content.

4. The water-resistant catalyst according to claim 1 or 2, characterized in that: The noble metal is palladium.

5. The method for preparing the water-resistant catalyst according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: S1, dispersing a cerium precursor and rod-shaped titanium dioxide in a solvent, then adding a precipitant to the obtained dispersion and stirring evenly to obtain a mixed solution; S2, heating the mixed solution and performing a reflux reaction, cooling the mixed solution to room temperature after the reflux reaction is completed, separating the obtained reaction solution into solid and liquid, and drying and calcining the solid product to obtain a composite oxide support; S3, dispersing the composite oxide carrier and the active component precursor in a solvent, evaporating the solvent in the obtained dispersion and then calcining to obtain the water-resistant catalyst.

6. The method for preparing the water-resistant catalyst according to claim 5, characterized in that: In step S1, the cerium precursor is selected from at least one of cerium nitrate, cerium chloride and cerium sulfate; and the precipitant is urea and / or hexamethylenetetramine.

7. The method for preparing the water-resistant catalyst according to claim 5, characterized in that: In step S2, the conditions for the reflux reaction include a temperature of 70-100°C and a time of 2-10 hours; the conditions for the drying include a temperature of 100-130°C and a time of 3-12 hours; and the conditions for the calcination include a temperature of 300-900°C and a time of 3-6 hours.

8. The method for preparing the water-resistant catalyst according to claim 5, characterized in that: In step S3, the active component precursor is selected from at least one of palladium nitrate, palladium chloride and palladium sulfate; the calcination conditions include a temperature of 300-900° C. and a time of 3-6 hours.

9. Use of the water-resistant catalyst according to any one of claims 1 to 4 in low-concentration methane oxidation.