A betaine type polysiloxane, preparation method and application thereof

Through the preparation of betaine-type polysiloxane, the problems of poor high temperature resistance and poor inhibitory performance of shale inhibitors are solved, efficient shale hydration inhibition and well wall stability improvement are achieved, and the preparation process is simplified and Reduced costs.

CN116425979BActive Publication Date: 2024-10-11SOUTHWEST PETROLEUM UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310595079.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-10-11
Estimated Expiration
2043-05-24

AI Technical Summary

Technical Problem

Existing shale inhibitors have poor high-temperature resistance, poor inhibition performance, and complex preparation methods.

Method used

Betaine-type polysiloxane is used, which consists of octamethylcyclotetrasiloxane, tetramethyltetrahydrocyclotetrasiloxane, hexamethyldisiloxane, a first monomer, a second monomer, and a catalyst Polymerizes with initiators under acidic conditions to form inhibitors with high thermal and chemical stability, which are used in water-based drilling fluids to improve wellbore stability.

Benefits of technology

Betaine-type polysiloxane has good high temperature resistance and inhibitory properties. The molecular chain contains both anionic and cationic groups, which enhances the adsorption capacity with clay and forms a polymer film through hydrogen bonding. Effectively prevents hydration, reduces costs and simplifies the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116425979B_ABST
    Figure CN116425979B_ABST
Patent Text Reader

Abstract

The invention discloses a betaine type polysiloxane, a preparation method and an application thereof, and relates to the technical field of oilfield chemistry. The raw materials for preparing the polysiloxane include: octamethylcyclotetrasiloxane, tetramethyltetrahydrocyclotetrasiloxane, hexamethyldisiloxane, a first monomer, a second monomer, a catalyst, and an initiator. The preparation method comprises: taking the raw materials, polymerizing octamethylcyclotetrasiloxane, tetramethyltetrahydrocyclotetrasiloxane, hexamethyldisiloxane and an initiator under acidic conditions to obtain hydrogen-containing polysiloxane, and preparing tertiary amino polysiloxane with the hydrogen-containing polysiloxane and the first monomer under the action of a catalyst; quaternizing the tertiary amino polysiloxane and the second monomer, and distilling under reduced pressure to obtain a product. The invention also provides the application of betaine type polysiloxane in water-based drilling fluid shale inhibitors. The polymer has high thermal stability and chemical stability, good high temperature resistance, good inhibition performance, and a small amount can reduce costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oilfield chemistry, in particular to a betaine type polysiloxane, a preparation method thereof and application thereof. Background Art

[0002] Due to the increasing demand for oil resources, the study of unconventional shale gas has become a hot research topic. However, deep drilling operations face severe challenges due to factors such as high formation pressure, high temperature, and complex lithology. Oil-based drilling fluids are known for their lubricity, inhibition, and high-temperature stability, but their use is limited by their cost and environmental regulations. On the other hand, water-based drilling fluids have been widely used in drilling operations due to their environmental friendliness, significant rheological properties, and excellent performance. However, water-sensitive shale in the formation can swell by absorbing free water in the water-based drilling fluid, leading to problems such as fracture development, wellbore collapse, and economic losses. Therefore, a strongly inhibitory water-based drilling fluid system has become the focus of research, and the development of new high-performance shale inhibitors has become the key to the study of water-based drilling fluid systems.

[0003] The invention patent with publication number CN202210210471 discloses a method for preparing a fluorinated silicon polymer shale inhibitor for water-based drilling fluid. The inhibitor uses cage-shaped polysilsesquioxane silane monomers and fluorinated acrylate monomers, which can significantly change the wettability of the rock surface and transform hydrophilic shale into hydrophobic shale; it has good inhibition, can significantly reduce clay hydration expansion, and inhibit shale hydration dispersion. The inhibitor has good inhibition performance, but poor high temperature resistance, and the preparation process is cumbersome and costly. The invention patent with publication number CN201611193488 discloses a shale inhibitor organosilicon polymer for drilling fluid and its preparation method, which has strong adsorption and coating clay particles. It can effectively reduce the expansion coefficient of shale, reduce the slurrying rate of clay, inhibit the hydration dispersion of shale, improve the stability of the well wall, inhibit collapse, and effectively protect the oil and gas layer. The inhibitor has certain environmental friendliness, but poor temperature resistance and inhibition performance needs to be improved. Summary of the invention

[0004] The purpose of the present invention is to solve the problems of poor high temperature resistance, poor inhibition performance and complicated preparation method of existing shale inhibitors. The present invention provides a betaine-type polysiloxane shale inhibitor for water-based drilling fluid that can effectively reduce shale hydration, improve wellbore stability and has good high temperature resistance and a preparation method thereof.

[0005] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions:

[0006] A betaine type polysiloxane, wherein the raw materials for preparing the polysiloxane include: octamethylcyclotetrasiloxane, tetramethyltetrahydrocyclotetrasiloxane, hexamethyldisiloxane, a first monomer, a second monomer, a catalyst,

[0007] Initiator; The structural formula of the polysiloxane is as follows:

[0008] Furthermore, the general structural formula of the first monomer is Where R 1 , R 2 , R 3 , R 4 , R 5 Each is independently the same or different, branched or unbranched, aliphatic or aromatic hydrocarbon group having 1 to 20 carbon atoms.

[0009] Furthermore, the general structural formula of the second monomer is Any of the following, where R 6 , R 8 For halogen elements, R 7 , R 9 , R 10 are independently the same or different, branched or unbranched, aliphatic or aromatic hydrocarbon groups having 1 to 20 carbon atoms.

[0010] Furthermore, the catalyst is platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane.

[0011] Furthermore, the amount of the catalyst added is 0.3%-0.5%wt of the total weight of the monomers.

[0012] Furthermore, the initiator is a strongly acidic ion exchange resin.

[0013] The present invention also provides a method for preparing the above-mentioned betaine-type polysiloxane, comprising the following steps:

[0014] S1. providing octamethylcyclotetrasiloxane, tetramethyltetrahydrocyclotetrasiloxane, hexamethyldisiloxane, a first monomer, a second monomer, a catalyst and an initiator;

[0015] S2, taking octamethylcyclotetrasiloxane, tetramethyltetrahydrocyclotetrasiloxane, hexamethyldisiloxane and an initiator, polymerizing them under acidic conditions for a first preset time at a first temperature to obtain a hydrogen-containing polysiloxane;

[0016] S3, mixing the hydrogen-containing polysiloxane obtained in S2 with the first monomer, adding a catalyst, reacting for a second preset time at a second temperature, to obtain a tertiary amino polysiloxane;

[0017] S4, mixing the tertiary amino polysiloxane obtained in S3 with the second monomer, reacting for a third preset time, the reaction temperature is a third temperature, and distilling under reduced pressure to obtain a final product, betaine polysiloxane.

[0018] Furthermore, the first preset time is 12 to 48 hours, the second preset time is 12 to 24 hours, and the third preset time is 12 to 24 hours.

[0019] Furthermore, the first temperature is 60-90°C, the second temperature is 60-80°C, and the third temperature is 80-100°C.

[0020] The present invention also provides an application of the betaine polysiloxane, wherein the betaine polysiloxane is used as a shale inhibitor for water-based drilling fluids.

[0021] Compared with the prior art, the advantages of the present invention are:

[0022] 1. The betaine type polysiloxane involved in the present invention has a polymer main chain with silicon atoms and oxygen atoms as the skeleton, has high thermal stability and chemical stability, and has good high temperature resistance. At the same time, its molecular chain carries both anionic groups and cationic groups, and has good water solubility. Compared with traditional anionic polymer inhibitors, it has a stronger ability to adsorb negatively charged clay, and quaternary ammonium cations can effectively enhance the adsorption capacity of polymers on clay. Compared with traditional cationic polymer inhibitors, it has better rheological properties and adaptability to filtration loss and wall-building properties. Carboxyl anions can be adsorbed on the clay surface through hydrogen bonding to form a polymer film, which effectively prevents and delays the contact between water molecules and the clay surface to inhibit surface hydration.

[0023] 2. The method for preparing a betaine-type polysiloxane involved in the present invention is simple, has mild reaction conditions and is widely applicable.

[0024] 3. The betaine-type polysiloxane involved in the present invention has good temperature resistance and inhibition performance when used in shale inhibitors, and can achieve good performance with a small amount, greatly reducing the cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The present invention is a schematic diagram of the synthesis route of a betaine-type polysiloxane.

[0026] Figure 2 The infrared spectrum of the betaine polysiloxane involved in the present invention.

[0027] Figure 3 Schematic diagram of a linear expansion experiment of a betaine type polysiloxane involved in the present invention Figure 1 .

[0028] Figure 4 Schematic diagram of a linear expansion experiment of a betaine type polysiloxane involved in the present invention Figure 2 .

[0029] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0030] Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. DETAILED DESCRIPTION

[0031] The present invention provides a betaine type polysiloxane, and the raw materials for preparing the polysiloxane include: octamethylcyclotetrasiloxane, tetramethyltetrahydrocyclotetrasiloxane, hexamethyldisiloxane, a first monomer, a second monomer, a catalyst, and an initiator; the structural formula of the polysiloxane is as follows:

[0032] It is understandable that the betaine-type polysiloxane involved in the present invention has a polymer main chain with silicon atoms and oxygen atoms as the skeleton, has high thermal stability and chemical stability, and has good high temperature resistance. At the same time, its molecular chain carries both anionic groups and cationic groups, and has good water solubility. Compared with traditional anionic polymer inhibitors, it has a stronger ability to adsorb negatively charged clay, and quaternary ammonium cations can effectively enhance the adsorption capacity of polymers on clay. Compared with traditional cationic polymer inhibitors, it has better rheological properties and adaptability to filtration loss and wall-building properties. Carboxyl anions can be adsorbed on the clay surface through hydrogen bonding to form a polymer film, which effectively prevents and delays the contact between water molecules and the clay surface to inhibit surface hydration.

[0033] In certain embodiments of the present invention, the catalyst is platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane.

[0034] In certain embodiments of the present invention, the amount of the catalyst added is 0.3%-0.5%wt of the total weight of the monomers. Specifically, the amount of the catalyst added is preferably 0.5%wt of the total weight of the monomers.

[0035] In certain embodiments of the present invention, the initiator is a strongly acidic ion exchange resin.

[0036] In certain embodiments of the present invention, the general structural formula of the first monomer is Where R 1 , R 2 , R 3 , R 4 , R 5 Each is independently the same or different, branched or unbranched, aliphatic or aromatic hydrocarbon group having 1 to 20 carbon atoms.

[0037] In certain embodiments of the present invention, the first monomer is preferably N,N-dimethylallylamine.

[0038] In certain embodiments of the present invention, the general structural formula of the second monomer is

[0039] Any of the following, where R 6 , R 8 For halogen elements, R 7 , R 9 , R 10 are independently the same or different, branched or unbranched, aliphatic or aromatic hydrocarbon groups having 1 to 20 carbon atoms.

[0040] In certain embodiments of the present invention, the second monomer is preferably sodium chloroacetate.

[0041] The present invention also provides a method for preparing the above-mentioned betaine-type polysiloxane, comprising the following steps:

[0042] S1. providing octamethylcyclotetrasiloxane, tetramethyltetrahydrocyclotetrasiloxane, hexamethyldisiloxane, a first monomer, a second monomer, a catalyst and an initiator;

[0043] S2, taking octamethylcyclotetrasiloxane, tetramethyltetrahydrocyclotetrasiloxane, hexamethyldisiloxane and an initiator, polymerizing them under acidic conditions for a first preset time at a first temperature to obtain a hydrogen-containing polysiloxane;

[0044] S3, mixing the hydrogen-containing polysiloxane obtained in S2 with the first monomer, adding a catalyst, reacting for a second preset time at a second temperature, to obtain a tertiary amino polysiloxane;

[0045] S4, mixing the tertiary amino polysiloxane obtained in S3 with the second monomer, reacting for a third preset time, the reaction temperature is a third temperature, and distilling under reduced pressure to obtain a final product, betaine polysiloxane.

[0046] Specifically, in some embodiments,

[0047] S1, provide octamethylcyclotetrasiloxane (D 4 ), tetramethyltetrahydrocyclotetrasiloxane (D 4 H ), hexamethyldisiloxane (MM), a first monomer, a second monomer and a catalyst, wherein the first monomer is N,N-dimethylallylamine (DMAA), and the second monomer is sodium chloroacetate (SC);

[0048] S2. Octamethylcyclotetrasiloxane is subjected to ring-opening polymerization under acidic conditions to produce hydrogen-containing polysiloxane. The specific reaction conditions are as follows:

[0049] a) The reaction temperature is T = 60 ~ 90 ° C, the reaction time is t = 12 ~ 48h (the longer the reaction time, the greater the molecular weight of the polymer), and the reaction is carried out at N 2 Conducted in atmosphere;

[0050] b) The molar ratio of feed is D 4 :D 4 H :MM=6:2:1; the initiator is a strong acid ion exchange resin, and the amount added is 1wt% of the reaction system;

[0051] c) After the reaction is completed, the insoluble impurities are filtered to obtain a transparent liquid product, hydrogen-containing polysiloxane.

[0052] S3, the hydrogen-containing polysiloxane obtained in S2 and N, N-dimethylallylamine (DMAA) are reacted by hydrosilylation reaction in the presence of a catalyst to obtain a tertiary amino polysiloxane; specifically:

[0053] a) The reaction temperature is T = 60 ~ 80 ° C, the reaction time is t = 12 ~ 24h, the reaction is carried out in N 2 Conducted in atmosphere;

[0054] b) the mass ratio of the feed materials is hydrogen-containing polysiloxane: N, N-dimethylallylamine = 1:2.5, and the catalyst is platinum (0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane, and the amount added is 0.3% to 0.5% wt of the system;

[0055] c) After the reaction is completed, the liquid product tertiary amino polysiloxane is obtained by vacuum distillation.

[0056] S4, adding an initiator, subjecting the tertiary amino polysiloxane obtained in S3 to a quaternization reaction with sodium chloroacetate (SC), and performing reduced pressure distillation to obtain a final product, betaine type polysiloxane; specifically:

[0057] a) The reaction temperature is T = 80 ~ 100 ° C, t = 12 ~ 24h, the reaction is carried out under N 2 Conducted in atmosphere;

[0058] b) The molar ratio of the feed is betaine type polysiloxane: sodium chloroacetate = 1:1.2. First, sodium chloroacetate is dissolved in a small amount of pure water, and then isopropanol of the same weight as the system is added and mixed evenly, and then the betaine type polysiloxane is dripped into the sodium chloroacetate solution;

[0059] c) After the reaction is completed, the solvent is first removed by vacuum distillation; the product is then redissolved in an isopropanol solution, insoluble impurities are removed by centrifugation, and the isopropanol is removed by vacuum distillation again; anhydrous ethanol is then added to dissolve the remaining product, and the product is centrifuged again to remove trace impurities that may remain in the system, and the solvent is removed by rotary evaporation; anhydrous acetone is then added to the system, and after complete dissolution, the product is placed in a refrigerator freezer for freezing and crystallization, and the precipitated solid is vacuum dried at 85° C. for 3 hours to obtain a white solid final product, betaine-type polysiloxane.

[0060] It can be understood that the preparation method is simple, the reaction conditions are mild, and the applicability is wide.

[0061] In some embodiments of the present invention, the first preset time is 12 to 48 hours, the second preset time is 12 to 24 hours, and the third preset time is 12 to 24 hours.

[0062] In some embodiments of the present invention, the first temperature is 60-90°C, the second temperature is 60-80°C, and the third temperature is 80-100°C.

[0063] In some embodiments of the present invention, S2, S3 and S4 are all in N 2 Carried out in atmosphere.

[0064] The present invention also provides an application of the betaine polysiloxane, which is used for water-based drilling fluid shale inhibitor. When the betaine polysiloxane is used for shale inhibitor, it has good temperature resistance and inhibitory performance, and can achieve good performance with a small amount, which greatly reduces the cost.

[0065] Example 1

[0066] 1.1 Preparation and operation

[0067] See also Figure 1 , the specific operations are:

[0068] Providing octamethylcyclotetrasiloxane, tetramethyltetrahydrocyclotetrasiloxane, hexamethyldisiloxane, N,N-dimethylallylamine, sodium chloroacetate and catalyst;

[0069] S1. Octamethylcyclotetrasiloxane is subjected to ring-opening polymerization under acidic conditions to produce hydrogen-containing polysiloxane. The reaction conditions are as follows:

[0070] d) The reaction temperature is T = 60 ~ 90 ° C, the reaction time is t = 12 ~ 48h (the longer the reaction time, the greater the polymer molecular weight), the reaction is N 2 Conducted in atmosphere;

[0071] e) The molar ratio of feed is D 4 :D 4 H :MM=6:2:1; the initiator is a strong acid ion exchange resin, and the amount added is 1wt% of the reaction system;

[0072] f) After the reaction is completed, the insoluble impurities are filtered to obtain a transparent liquid product, hydrogen-containing polysiloxane.

[0073] S2, preparing tertiary amino polysiloxane by reacting the hydrogen-containing polysiloxane obtained in S1 with N,N-dimethylallylamine (DMAA) in the presence of a catalyst through a hydrosilylation reaction;

[0074] d) The reaction temperature is T = 60 ~ 80 ° C, the reaction time is t = 12 ~ 24h, the reaction is carried out under N 2 Conducted in atmosphere;

[0075] e) the mass ratio of the feed materials is hydrogen-containing polysiloxane: N, N-dimethylallylamine = 1:2.5, and the catalyst is platinum (0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane, and the amount added is 0.3% to 0.5% wt of the system;

[0076] f) After the reaction is completed, the liquid product tertiary amino polysiloxane is obtained by vacuum distillation.

[0077] S3, adding an initiator, subjecting the tertiary amino polysiloxane in S2 to a quaternization reaction with sodium chloroacetate (SC), and performing reduced pressure distillation to obtain the final product, betaine type polysiloxane.

[0078] c) The reaction temperature is T = 80 ~ 100 ° C, t = 12 ~ 24h, the reaction is carried out under N 2 Conducted in atmosphere;

[0079] d) The molar ratio of the feed is betaine type polysiloxane: sodium chloroacetate = 1:1.2. First, sodium chloroacetate is dissolved in a small amount of pure water, and then isopropanol of the same weight as the system is added and mixed evenly, and then the betaine type polysiloxane is dripped into the sodium chloroacetate solution;

[0080] e) After the reaction is completed, the solvent is first removed by vacuum distillation; the product is then redissolved in an isopropanol solution, insoluble impurities are removed by centrifugation, and the isopropanol is removed by vacuum distillation again; anhydrous ethanol is then added to dissolve the remaining product, and the product is centrifuged again to remove trace impurities that may remain in the system, and the solvent is removed by rotary evaporation; anhydrous acetone is then added to the system, and after complete dissolution, the product is placed in a refrigerator freezer for freezing and crystallization, and the precipitated solid is vacuum dried at 85° C. for 3 hours to obtain a white solid final product, betaine-type polysiloxane.

[0081] Experimental Example 1 Infrared Characterization of the Polymer Prepared in Example 1

[0082] 1.1 Test operation

[0083] The polymer prepared in Example 1 was characterized by infrared spectroscopy. Figure 2 .

[0084] 1.2 Results Analysis

[0085] See also Figure 2 It can be known that Figure 2 Wavenumbers in the figure is the wave number), 2700cm -1 ~2850cm -1 A new absorption peak appears at -N(CH 3 ) 2 The methyl absorption peak of 1630cm- 1 A new absorption peak appears at 2700cm -1 ~2850cm -1 There is no absorption peak at , indicating that the tertiary amine group is successfully quaternized and the final product, betaine-type polysiloxane, is successfully synthesized.

[0086] Experimental Example 2: Linear expansion test of the polymer prepared in Example 1

[0087] 2.1 Test operation

[0088] Experimental group 1 was set up as a control group of pure water, experimental group 2 was set up as a control group of 5% KCl solution, and experimental group 3 was set up as a control group of 1% commercial polyamine inhibitor.

[0089] The betaine polysiloxane prepared in Example 1 was used to prepare a 0.5% betaine polysiloxane inhibitor solution, 10 g of dried evaluation soil was pressed at a pressure of 10 MPa for 5 min, and then immersed in the prepared inhibitor solution to form Experimental Group 4. 1.0% betaine polysiloxane was prepared as Experimental Group 5, 1.5% betaine polysiloxane was prepared as Experimental Group 6, and 2% betaine polysiloxane was prepared as Experimental Group 7.

[0090] A linear expansion instrument was used to test the expansion of each experimental group for 16 hours. The expansion diagram is shown in Figure 3 and Figure 4 , and calculate the expansion rate. The expansion rate results are shown in Table 1.

[0091] Table 1

[0092] Group Solution Temperature / ℃ Expansion rate / % Experimental Group 1 Shimizu 25 20.65 Experimental Group 2 5% KCl 25 18.42 Experimental Group 3 1% Commercial polyamine inhibitor 25 15.51 Experimental Group 4 0.5% Betaine polysiloxane 25 14.13 Experimental Group 5 1.0% Betaine polysiloxane 25 13.19 Experimental Group 6 1.5% Betaine polysiloxane 25 12.85 Experimental Group 7 2.0% Betaine polysiloxane 25 12.30

[0093] 2.2 Results Analysis

[0094] Referring to Table 1, the expansion rates of the four experimental groups 4 to 7 of the betaine polysiloxane involved in the present invention are all below 14.13%, which is relatively low. The expansion rate of the commercial polyamine inhibitor is 15.51%, and the expansion rate of the traditional inorganic salt inhibitor KCl is 18.42%. It can be seen that the expansion rates of the other groups are relatively high. Comparing the experimental group 5: 1% betaine polysiloxane (expansion rate is 13.19%) and the experimental group 3: 1% commercial polyamine inhibitor (expansion rate is 15.51%), it can be seen that the betaine polysiloxane has a better inhibitory effect at the same concentration.

[0095] See also Figure 3 and Figure 4 The betaine polysiloxane experimental group of the present invention has a lower linear expansion rate than the control group of clear water, the control group of 5% KCl solution, and the control group of 1% commercial polyamine inhibitor. This advantage becomes more obvious over time.

[0096] It can be seen that the betaine-type polysiloxane shale inhibitor involved in the present invention has a low expansion rate and has an excellent inhibitory effect.

[0097] Experimental Example 3 Rolling recovery experiment of the polymer prepared in Example 1

[0098] 3.1 Test operation

[0099] Experimental group 1 was set up as a control group of pure water, experimental group 2 was set up as a control group of 5% KCl solution, and experimental group 3 was set up as a control group of 1% commercial polyamine inhibitor.

[0100] The betaine polysiloxane prepared in Example 1 was used to prepare a 0.5% betaine polysiloxane inhibitor solution, 10 g of dried evaluation soil was pressed at a pressure of 10 MPa for 5 min, and then immersed in the prepared inhibitor solution to form Experimental Group 4. 1.0% betaine polysiloxane was prepared as Experimental Group 5, 1.5% betaine polysiloxane was prepared as Experimental Group 6, and 2% betaine polysiloxane was prepared as Experimental Group 7.

[0101] 400mL of each solution with different concentrations was added to the aging tank, and 20g of 6-10 mesh dry rock chips were weighed and added to the aging tank. After rolling at 180℃ and 220℃ for 16h, the rock chips were sieved with a 40-mesh standard sieve and dried at 105℃ for 4h before weighing. The rock chip rolling recovery rate is: The experimental results of the cuttings rolling recovery at 180°C for each group are shown in Table 2, and the experimental results of the cuttings rolling recovery at 220°C for each group are shown in Table 3.

[0102] Table 2. Results of the cuttings rolling recovery experiment at 180°C

[0103] Group Solution Temperature / ℃ Rolling recovery rate / % Experimental Group 1 Shimizu 180 13.21 Experimental Group 2 5% KCl 180 22.46 Experimental Group 3 1.0% Commercial polyamine inhibitor 180 57.93 Experimental Group 4 0.5% Betaine polysiloxane 180 78.58 Experimental Group 5 1.0% Betaine polysiloxane 180 84.07 Experimental Group 6 1.5% Betaine polysiloxane 180 90.14 Experimental Group 7 2.0% Betaine polysiloxane 180 94.56

[0104] Table 3. Results of the rock cuttings rolling recovery experiment at 220°C

[0105] Group Solution Temperature / ℃ Rolling recovery rate / % Experimental Group 1 Shimizu 220 6.35 Experimental Group 2 5% KCl 220 14.31 Experimental Group 3 1.0% Commercial polyamine inhibitor 220 46.24 Experimental Group 4 0.5% Betaine polysiloxane 220 71.29 Experimental Group 5 1.0% Betaine polysiloxane 220 78.85 Experimental Group 6 1.5% Betaine polysiloxane 220 82.41 Experimental Group 7 2.0% Betaine polysiloxane 220 87.01

[0106] Refer to Table 3 and Table 4 above to see that at 180°C, compared with the clean water of Experimental Group 1, the rolling recovery rates of Experimental Groups 4 to 6 after adding betaine polysiloxane to the cuttings were significantly improved, all above 78.58%, while the rolling recovery rate of the clean water group was only 6.35%, the rolling recovery rate of the traditional inorganic salt inhibitor KCl was only 14.31%, and the rolling recovery rate of the commercial polyamine inhibitor was only 46.24%. Moreover, at a high temperature of 220°C, the betaine polysiloxane involved in the present invention still has a good inhibitory effect, and the rolling recovery rate of the cuttings can reach up to 87% and the lowest is 71.29%, which is much higher than the recovery rates of the other three groups.

[0107] It can be seen that the betaine polysiloxane involved in the present invention has good high temperature resistance and good inhibition performance.

[0108] In summary, the betaine-type polysiloxane provided by the present invention has good temperature resistance and inhibition performance when used in shale inhibitors, and can achieve good performance even with a small amount. Compared with commercial polyamine inhibitors and traditional inorganic salt inhibitor KCl, it has better inhibition effect and better high temperature resistance, and has great advantages.

[0109] The above embodiment is only one implementation of the present invention, and its description is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.

Claims

1. Application of betaine type polysiloxane, It is characterized in that The betaine-type polysiloxane is used for a water-based drilling fluid shale inhibitor. The raw materials for preparing the polysiloxane include: octamethylcyclotetrasiloxane, tetramethyltetrahydrocyclotetrasiloxane, hexamethyldisiloxane, a first monomer N,N-dimethylallylamine, a second monomer sodium chloroacetate, a catalyst, and an initiator.

2. The use of a betaine polysiloxane according to claim 1, It is characterized in that The catalyst is platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane.

3. The use of a betaine polysiloxane according to claim 2, It is characterized in that The added amount of the catalyst is 0.3% to 0.5%wt of the total weight of the monomers.

4. The use of a betaine polysiloxane according to claim 1, It is characterized in that The initiator is a strongly acidic ion exchange resin.

5. The use of a betaine polysiloxane according to claim 1, It is characterized in that The preparation method of the betaine type polysiloxane comprises the following steps: S1. providing octamethylcyclotetrasiloxane, tetramethyltetrahydrocyclotetrasiloxane, hexamethyldisiloxane, a first monomer, a second monomer, a catalyst and an initiator; S2, taking octamethylcyclotetrasiloxane, tetramethyltetrahydrocyclotetrasiloxane, hexamethyldisiloxane and an initiator, polymerizing them under acidic conditions for a first preset time at a first temperature to obtain a hydrogen-containing polysiloxane; S3, mixing the hydrogen-containing polysiloxane obtained in S2 with the first monomer, adding a catalyst, reacting for a second preset time at a second temperature, to obtain a tertiary amino polysiloxane; S4, mixing the tertiary amino polysiloxane obtained in S3 with the second monomer, reacting for a third preset time, the reaction temperature is a third temperature, and distilling under reduced pressure to obtain a final product, betaine polysiloxane.

6. Use of a betaine type polysiloxane according to claim 5, It is characterized in that The first preset time is 12 to 48 hours, the second preset time is 12 to 24 hours, and the third preset time is 12 to 24 hours.

7. Use of a betaine polysiloxane according to claim 5, It is characterized in that The first temperature is 60-90°C, the second temperature is 60-80°C, and the third temperature is 80-100°C.