Sound absorbing materials
By capturing small-diameter resin particles inside the fiber blocks and configuring large-diameter resin particles between the fiber blocks, the problem of insufficient sound absorption performance of existing sound-absorbing materials in the low and high frequency ranges is solved, and excellent sound absorption effect is achieved over a wide frequency range.
Patent Information
- Application Number
- CN202080106536.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-10-29
AI Technical Summary
Existing sound-absorbing materials struggle to exhibit excellent sound absorption performance in both low and high frequency ranges simultaneously. In particular, while improving sound absorption performance in the high frequency range, sound absorption performance in the low frequency range is often insufficient.
The sound-absorbing material is made of fiber blocks, in which first resin particles are captured inside the fiber blocks and second resin particles are arranged between the fiber blocks. The particle size of the first resin particles is smaller than that of the second resin particles. This structural design improves the sound absorption performance in the low-frequency and high-frequency ranges.
It achieves excellent sound absorption performance in both low and high frequency ranges, improving the sound absorption effect of sound-absorbing materials in the frequency range.
Smart Images

Figure CN116438340B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a sound absorbing material used for noise countermeasures of electric equipment, automobiles, and the like. Background Art
[0002] The noise generated by electrical equipment such as air conditioners, refrigerators, and automobiles includes sound waves in the low-frequency range and the high-frequency range, so a sound-absorbing material having a wide range of sound-absorbing performance from the low-frequency range to the high-frequency range is required. So far, a sound-absorbing material is known in which a porous material such as glass wool is attached with a powder material such as polyurethane resin. Patent document 1 discloses the following technology: a porous material with a fine powder material attached is formed into a sheet of a certain thickness to improve the sound-absorbing performance in the high-frequency range.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Publication No. 2019-44548 (see Table 1, Figure 3 wait) Summary of the invention
[0006] Problems to be solved by the invention
[0007] However, although the sound absorption performance in the high frequency range can be improved by appropriately selecting the particle size of the fine powder material attached to the porous material, it is difficult to improve the sound absorption performance in the low frequency range. Therefore, it is a problem to obtain a sound absorbing material that improves the sound absorption performance in the high frequency range and the sound absorption performance in the low frequency range.
[0008] The present disclosure has been made to solve the above-mentioned problems, and an object of the present disclosure is to provide a sound absorbing material having excellent sound absorbing performance in low-frequency ranges and high-frequency ranges.
[0009] Means for solving problems
[0010] The sound absorbing material of the present disclosure includes: a fiber block in which one or more fibers are entangled with each other to form a block, and the block has a first void inside and a first resin particle captured in the first void; and a second resin particle, which is arranged in the second void formed between the plurality of fiber blocks and has a larger particle size than the first resin particle.
[0011] Effects of the Invention
[0012] According to the present disclosure, the first resin particles captured in the first gaps improve the sound absorption performance in the high-frequency range, and the second resin particles arranged in the second gaps and having a particle size larger than that of the first resin particles improve the sound absorption performance in the low-frequency range. Therefore, a sound absorbing material having excellent sound absorption performance in the low-frequency range and the high-frequency range can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a cross-sectional schematic diagram showing a schematic structure of the sound absorbing material in the first embodiment.
[0014] Figure 2 It is a schematic cross-sectional view showing the structure of the fiber block of the sound absorbing material in the first embodiment.
[0015] Figure 3 It is a graph showing the sound absorption rate of the sound absorbing material in Embodiment 1.
[0016] Figure 4 Graph showing the particle size ratio dependency of the sound absorption rate of the sound absorbing material in the second embodiment.
[0017] Figure 5 This is a graph showing the dependence of the sound absorption rate of the sound absorbing material in the second embodiment on the particle size of the second resin particles.
[0018] Figure 6 Graph showing the fiber block diameter dependence of the sound absorption rate of the sound absorbing material in the third embodiment.
[0019] Figure 7 Graph showing the volume density dependency of the sound absorption rate of the sound absorbing material in the fourth embodiment.
[0020] Figure 8 It is a cross-sectional schematic diagram showing a schematic structure of a sound absorbing material in the fifth embodiment. DETAILED DESCRIPTION
[0021] The present inventors have conducted intensive studies and have found that a sound absorbing material having excellent sound absorbing performance in both low-frequency ranges and high-frequency ranges can be obtained by using a structure in which fiber blocks that capture fine resin particles in fibers and coarse resin particles exist between a plurality of fiber blocks, thereby achieving a structure that improves the sound absorbing performance in a wide frequency range.
[0022] Hereinafter, embodiments of the present disclosure will be described in detail based on the drawings.
[0023] Implementation method 1.
[0024] Figure 1 Schematic cross-sectional view of the sound absorbing material 1 according to Embodiment 1. The sound absorbing material 1 is configured such that first resin particles 3 are captured in each of a plurality of fiber clumps 2, and second resin particles 4 having a larger diameter than the first resin particles 3 are arranged in second gaps 9 between the plurality of fiber clumps 2.
[0025] like Figure 2As shown, as for the fiber block 2, a block is formed by entanglement of one or more fibers 6, and the first resin particles 3 are captured in the first voids 8 formed inside the block, thereby forming a fiber block 2. The fiber block 2 is a block such as a spherical block formed by bending one fiber 6 or making a plurality of fibers 6 dense. The fiber block 2 may be an elliptical, polygonal, etc., or a flat shape in which a part of their shape is flat. All of the plurality of fiber blocks 2 may be of one shape, or a plurality of shapes may be mixed, such as a mixture of spherical and flat shapes. The fiber block 2 may be a size that allows the first resin particles 3 to be captured in the first voids 8 and allows the second voids 9 to be formed in which the second resin particles having a larger particle size than the first resin particles 3 can be configured. For example, the diameter of the fiber block 2 may be about 0.1 mm or more and about 100 mm or less. Among them, the so-called diameter of the fiber block 2 refers to the average diameter, for example, measured at about 20 locations using a vernier caliper and calculated by arithmetic averaging.
[0026] The fiber 6 may be selected from one or more inorganic fiber materials such as glass wool, rock wool, carbon fiber, alumina fiber, wollastonite, potassium titanate fiber, natural fiber materials such as cotton and hemp, polyester resin fiber, aramid resin fiber, and other organic fiber materials. The wire diameter of the fiber 6 may be determined from the viewpoint of appropriately forming the first void 8 for capturing the first resin particles 3, and may be, for example, greater than 0.1 μm and less than 10 μm. The wire diameter of the fiber 6 is obtained, for example, by measuring the average value of about 20 points in a cross-sectional image of the fiber 6 magnified by about 1000 to 5000 times using a SEM (scanning electron microscope).
[0027] The first resin particles 3 may be selected from one or more of polyurethane resin, phenolic resin, epoxy resin, acrylic resin, polyester resin, polyamide resin, melamine resin, etc. The particle size of the first resin particles 3 may be set to a size that obtains sound absorption performance in the high-frequency range and allows the first resin particles 3 to be captured by the first voids 8. The size of the first voids 8 can be adjusted by changing the wire diameter of the fiber 6 according to the particle size of the first resin particles 3. For example, when the particle size of the first resin particles 3 is 1 mm, the wire diameter of the fiber 6 can be 7 μm. The particle size of the first resin particles 3 refers to the average particle size, which is obtained by measuring the particle size of the first resin particles 3 captured at about 20 locations in an image of the surface or cross section of the fiber block 2 magnified by about 1000 to 5000 times using SEM, and performing arithmetic averaging.
[0028] The second voids 9 are provided between the plurality of fiber blocks 2. The size of the second voids 9 and the total volume occupied in the sound absorbing material 1 are related to the size of the fiber blocks 2. When the filling amount of the fiber blocks 2 is the same, if the fiber blocks 2 become smaller, the proportion of the total volume of the second voids 9 occupied in the sound absorbing material 1 in the same volume becomes larger. If the second voids 9 become larger, the second resin particles 4 having a large particle size can be arranged in the second voids 9. In addition, by dispersing the fiber blocks 2, the second resin particles 4 can be dispersedly arranged.
[0029] The second resin particles 4 may be selected from one or more of polyurethane resin, phenolic resin, epoxy resin, acrylic resin, polyester resin, polyamide resin, melamine resin, etc. If coarse particles are used for the second resin particles 4, the vibration energy of the sound waves in the low-frequency range is effectively converted into heat energy, so that the sound absorption performance in the low-frequency range can be improved. Therefore, resin particles having a larger particle size than the first resin particles 3 are used for the second resin particles 4. For example, when the particle size of the first resin particles 3 is 0.6 mm and the diameter of the fiber block 2 is 26 mm, the particle size of the second resin particles 4 can be 21 mm. The so-called particle size of the second resin particles 4 refers to the average particle size, which is obtained by, for example, measuring about 20 places using an optical microscope or a vernier caliper and taking the arithmetic average.
[0030] From the viewpoint of capturing the first resin particles 3 in the first voids 8 and arranging the second resin particles 4 in the second voids 9, the weight ratio of the fiber block 2 to the total weight of the resin particles including the first resin particles 3 and the second resin particles 4 may be 70:30 to 95:5. Preferably, it may be 80:20 to 90:10. If it is 80:20 to 90:10, the first resin particles 3 can be effectively captured in the first voids 8 and the second resin particles 4 can be effectively arranged in the second voids 9. In addition, the weight ratio of the first resin particles 3 to the second resin particles 4 may be 5:95 to 50:50. Preferably, it may be 20:80 to 40:60. If it is 20:80 to 40:60, the second resin particles 4 can be easily arranged in the second voids 9 in a dispersed manner.
[0031] The total resin particle content ratio, i.e., the ratio of the total resin particle weight in the sound absorbing material 1, can be verified by heat-treating and ashing the mixture of the first resin particles 3 and the second resin particles 4 at about 400 to 500° C. when the inorganic fiber material is used in the fiber block 2. Specifically, the total resin particle content ratio can be determined from the weight before the heat treatment (W before ) and the weight after heat treatment (W after ), calculated using the following formula 1.
[0032] Total resin particle content = (1-W after / W before)×100···(Formula 1)
[0033] In addition, when the fiber block 2, the first resin particles 3 and the second resin particles 4 are placed in, for example, a bag-shaped packaging material 5, the volume density of the sound absorbing material 1 can be calculated using the following formula 2 from the volume of the bag-shaped packaging material 5 and the total weight of the filling material including the fiber block 2, the first resin particles 3 and the second resin particles 4.
[0034] The volume density of the sound absorbing material 1 = the total weight of the filling material ÷ the volume of the packaging material 5 (Formula 2)
[0035] Among them, the packaging material 5 is not limited to a bag-shaped one, and a sheet-shaped packaging material can be used. By using the packaging material 5, it is possible to prevent the fibers 6, the first resin particles 3, and the second resin particles 4 from scattering. The packaging material 5 may have ventilation openings to the extent that the sound incident on the sound absorbing material 1 from the outside is not reflected and the fibers 6, the first resin particles 3, and the second resin particles 4 are not scattered. Specifically, glass cloth, non-woven fabrics, synthetic fiber cloth, etc. can be used. They can be used individually, one can be overlapped, and multiple combinations can be overlapped. In particular, when the sound absorbing material 1 is used indoors, etc. to prevent the scattering of the fibers 6, the first resin particles 3, and the second resin particles 4, it is preferred to use multiple overlapping ones. In addition, it is also possible to directly configure and use it in the gap between the object generating noise, etc. without using the packaging material 5. In this case, the volume density of the sound absorbing material 1 can be obtained by replacing the volume of the gap between the object with the volume of the packaging material 5.
[0036] Next, a test piece of the sound absorbing material 1 of the present embodiment was prepared, and the evaluation results of the sound absorbing performance will be described. In the evaluation of the sound absorbing performance, the sound absorption coefficient of each sound absorbing material 1 was measured using a sound absorption coefficient measuring instrument by the vertical incidence method described in JIS A1405-2:2007, and then the relative value of the sound absorption coefficient of each sound absorbing material 1 was calculated based on the sound absorption coefficient of the sound absorbing material 1 of Comparative Example 1 at a frequency f of 500 Hz and 1000 Hz, and the relative value of the sound absorption coefficient of each sound absorbing material 1 was compared.
[0037] <Example 1>
[0038] As the first resin particles 3, polyurethane resin particles with a particle size of 0.6 mm and a total weight of 0.84 g were prepared, and as the second resin particles 4, polyurethane resin particles with a particle size of 21 mm and a total weight of 1.96 g were prepared. As the fibers 6, glass wool with a line diameter of 4 μm was used, and a plurality of fiber blocks 2 in which the first resin particles 3 were captured were formed, and the second resin particles 4 were arranged around the fiber blocks 2 to prepare a test piece. The test piece with a total weight of 18.8 g was placed in a glass cloth bag-shaped packaging material 5 with a diameter of 100 mm and a thickness of 25 mm, which was circular when viewed from above, to obtain a volume density of 96 kg / m 3Sound absorbing material 1.
[0039] <Comparative Example 1>
[0040] As a comparative example, a sound absorbing material 1 was obtained in the same manner as in Example 1 without adding the first resin particles 3 and the second resin particles 4 .
[0041] <Comparative Example 2>
[0042] The total weight of the first resin particles 3 was set to 2.8 g, and the sound absorbing material 1 was obtained in the same manner as in Example 1 without adding the second resin particles 4 .
[0043] The conditions of Example 1, Comparative Example 1 and Comparative Example 2 are shown in Table 1 below.
[0044] [Table 1]
[0045] Example 1 Comparative Example 1 Comparative Example 2 First resin particles have none have Second resin particles have none none
[0046] Figure 3 This is a graph comparing the relative values of the sound absorption rate produced by the presence or absence of the first resin particles 3 and the second resin particles 4. Figure 3 It can be seen that the sound absorbing material 1 of Example 1 including the first resin particles 3 and the second resin particles 4 has a superior sound absorption rate compared with the sound absorbing material 1 of Comparative Example 1 to which the first resin particles 3 and the second resin particles 4 are not added, and the sound absorbing material 1 of Comparative Example 2 to which the first resin particles 3 are added but the second resin particles 4 are not added.
[0047] At 500 Hz, which is a low frequency range, the relative value of the sound absorption rate of Example 1 is 1.96, which is improved compared to 1 of Comparative Example 2, indicating the effect of the second resin particles 4. In addition, at 1000 Hz, which is a high frequency range, the relative value of the sound absorption rate of Example 1 is 1.15, which is improved compared to 1 of Comparative Example 2, indicating that even if the second resin particles 4 are provided, the sound absorption rate in the high frequency range does not decrease.
[0048] In this way, by forming the fiber blocks 2 that capture the first resin particles 3 in the first gaps 8, and arranging the second resin particles 4 having a particle size larger than that of the first resin particles in the second gaps 9 formed using the plurality of fiber blocks 2, it is possible to obtain a sound absorbing material 1 having excellent sound absorbing performance in both the low-frequency range and the high-frequency range.
[0049] In addition, although the example of entanglement of one or more fibers 6 to form a block for making the fiber block 2 is shown, the block may be made by cutting a mat-shaped molded product. By cutting and using the mat-shaped molded product, a fiber block 2 of a desired size can be made. For cutting, various cutting machines such as a knife cutter, a hammer rotary cutter, a roller rotary cutter, and a pin disk rotary cutter can be used.
[0050] In addition, it is preferable that the fiber lumps 2 and the second resin particles 4 are uniformly dispersed throughout the entire sound absorbing material 1. When the fiber lumps 2 and the second resin particles 4 are uniformly dispersed, it is easy to form a structure that is effective for sound absorption of sound waves in the low frequency range and a structure that is effective for sound absorption of sound waves in the high frequency range in the entire sound absorbing material 1, thereby suppressing the reduction in sound absorption performance due to individual differences. In addition, the second resin particles 4 may be non-uniform as long as the sound absorption performance is not significantly reduced.
[0051] In addition, the first voids 8 can be provided by entanglement of the fibers 6 three-dimensionally, and the volume density of the sound absorbing material 1 can be adjusted to an appropriate range by the amount of the first voids 8. If the volume density is set to an appropriate range, when the fiber block 2 and the second resin particle 4 are mixed, the first resin particle 3 is easily captured by the first voids 8, and a plurality of incident paths of sound waves can be formed in the sound absorbing material 1, so that the sound absorbing material 1 has a structure that is easy to absorb sound. The size of the first voids 8 is related to the linear diameter and density of the fiber 6. When the linear diameter of the fiber 6 is reduced and the density is increased, the first voids 8 are reduced. If the first voids 8 are reduced, the first resin particles 3 are easily captured by the first voids 8.
[0052] In the production of the sound absorbing material 1 of the present embodiment, the fiber mass 2 in which the first resin particles 3 are captured and the second resin particles 4 are mixed, and by mixing the mass formed by the mutual entanglement of the first resin particles 3, the second resin particles 4, and the fibers 6, the first resin particles 3 are captured in the mass to form the fiber mass 2, and the second resin particles 4 are arranged between the plurality of fiber mass 2. In this case, the particle size of the second resin particles 4 may be adjusted so as not to prevent the capture of the second resin particles 4 by the first voids 8 and the capture of the first resin particles 3 by the first voids 8.
[0053] Implementation method 2.
[0054] In Embodiment 1, an example of comparing the presence or absence of the first resin particles 3 and the second resin particles 4 is shown. In this embodiment, an example of changing the particle size of the second resin particles 4 and changing the ratio of the particle sizes is described. The other configurations are the same as those in Embodiment 1. The sound absorbing performance is evaluated by the same method as in Embodiment 1.
[0055] Hereinafter, the ratio of the particle diameter of the second resin particle 4 to the particle diameter of the first resin particle 3 is referred to as a particle diameter ratio. The particle diameter ratio can be calculated using the following formula 3 from the particle diameter (R1) of the first resin particle 3 and the particle diameter (R2) of the second resin particle 4.
[0056] Particle size ratio = R2 ÷ R1 (Formula 3)
[0057] <Example 2>
[0058] A sound absorbing material 1 was obtained in the same manner as in Example 1 except that the particle diameter of the second resin particles 4 was 5 mm and the particle diameter ratio was 8.
[0059] <Example 3>
[0060] The sound absorbing material 1 was obtained in the same manner as in Example 1 except that the particle diameter of the second resin particles 4 was 13 mm and the particle diameter ratio was 22.
[0061] <Example 4>
[0062] The sound absorbing material 1 was obtained in the same manner as in Example 1 except that the particle diameter of the second resin particles 4 was 32 mm and the particle diameter ratio was 53.
[0063] The evaluation results are shown in Table 2. For reference, the evaluation results of Example 1 are shown again.
[0064] [Table 2]
[0065] Example 1 Example 2 Example 3 Example 4 Particle size ratio 35 8 22 53 Frequency (500Hz) 1.96 1.69 1.92 2.02 Frequency (1000Hz) 1.15 1.20 1.17 1.11
[0066] The sound absorption coefficients of Examples 1 to 4 are converted into coordinates. Figure 4 It can be seen that even if the particle size ratio is changed, it still has excellent sound absorption. Figure 4 The dotted line in is an auxiliary line showing the behavior of the relative value of the sound absorption rate with respect to each particle diameter ratio.
[0067] At 500 Hz, which is a low frequency range, the relative values of the sound absorption rate of Example 2 with a particle diameter ratio of 8, Example 3 with a particle diameter ratio of 22, and Example 4 with a particle diameter ratio of 53 are 1.69, 1.92, and 2.02, respectively, which are improved relative to 1 of the above-mentioned Comparative Example 2. In addition, at 1000 Hz, which is a high frequency range, the relative values of the sound absorption rate of Example 2, Example 3, and Example 4 are 1.20, 1.17, and 1.11, respectively, which are improved relative to 1 of Comparative Example 2, indicating that even if the particle diameter of the second resin particles 4 is changed, the sound absorption rate in the high frequency range does not decrease.
[0068] In addition, if Figure 4 As shown, when the particle size ratio is increased, the second resin particles 4 are difficult to be captured by the first voids 8 inside the fiber block 2, and are easily dispersed in the second voids 9 which are the voids between the plurality of fiber blocks 2. Therefore, the particle size ratio can be greater than 2, preferably greater than 8, and more preferably greater than 22.
[0069] In this way, even if the particle size ratio is changed, a sound absorbing material 1 having excellent sound absorbing performance in both the low frequency range and the high frequency range can be obtained. When the particle size ratio is increased, the second resin particles 4 are less likely to be captured by the first voids 8 and are easily dispersed in the second voids 9, so that a sound absorbing material 1 having excellent sound absorbing performance in both the low frequency range and the high frequency range can be obtained.
[0070] In addition, although the example in which the particle diameter ratio is adjusted by changing the particle diameter of the second resin particles 4 is shown in this embodiment, the particle diameter ratio may be adjusted by changing the particle diameter of the first resin particles 3 .
[0071] In addition, if Figure 5 As shown, the particle size of the second resin particles 4 is preferably 1 mm or more, more preferably 5 mm or more, and even more preferably 13 mm or more from the viewpoint of improving the sound absorbing performance in the low frequency range.
[0072] Implementation method 3.
[0073] In this embodiment, an example in which the diameter of the fiber block 2 is changed will be described. The other configurations are the same as those of the first embodiment. The sound absorbing performance is evaluated by the same method as that of the first embodiment.
[0074] <Example 5>
[0075] A sound absorbing material 1 was obtained in the same manner as in Example 1 except that the diameter of the fiber block 2 was set to 12 mm.
[0076] <Example 6>
[0077] The sound absorbing material 1 was obtained in the same manner as in Example 1 except that the diameter of the fiber block 2 was set to 49 mm.
[0078] <Example 7>
[0079] The sound absorbing material 1 was obtained in the same manner as in Example 1 except that the diameter of the fiber block 2 was set to 68 mm.
[0080] The evaluation results are shown in Table 3. For reference, the evaluation results of Example 1 are shown again.
[0081] [Table 3]
[0082] Example 1 Example 5 Example 6 Example 7 Diameter of fiber block [mm] 26 12 49 68 Frequency (500Hz) 1.96 1.94 1.86 1.67 Frequency (1000Hz) 1.15 1.17 1.16 1.15
[0083] The sound absorption coefficients of Example 1 and Example 5 to Example 7 are converted into coordinates. Figure 6 It can be seen that even if the diameter of the fiber block 2 is changed, it still has excellent sound absorption. Figure 6 The dotted line in FIG. 8 is an auxiliary line showing the behavior of the relative value of the sound absorption coefficient with respect to each diameter.
[0084] At 500 Hz, which is a low frequency range, the relative values of the sound absorption rate of Example 5, which has a diameter of 12 mm, Example 6, which has a diameter of 49 mm, and Example 7, which has a diameter of 68 mm, are 1.94, 1.86, and 1.67, respectively, which are improved relative to 1 of Comparative Example 2. In addition, at 1000 Hz, which is a high frequency range, the relative values of the sound absorption rate of Example 5, Example 6, and Example 7 are 1.17, 1.16, and 1.15, respectively, which are improved relative to 1 of Comparative Example 2, indicating that even if the diameter of the fiber block 2 is changed, the sound absorption rate in the high frequency range does not decrease.
[0085] When the diameter of the fiber mass 2 exceeds 70 mm, the proportion of the second voids 9 occupied in the sound absorbing material 1 becomes small, and it may be difficult to arrange the second resin particles 4 in the second voids 9. On the other hand, when the diameter of the fiber mass 2 is less than 5 mm, the filler including the fiber mass 2, the first resin particles 3, and the second resin particles 4 is densely filled in the sound absorbing material 1, and sometimes the incidence of sound waves to the sound absorbing material 1 is blocked. Therefore, the diameter of the fiber mass 2 is preferably 5 mm or more and 70 mm or less, more preferably 10 mm or more and 50 mm or less, and further preferably 20 mm or more and 40 mm or less.
[0086] In this way, even if the diameter of the fiber mass 2 is changed, a sound absorbing material 1 having excellent sound absorbing performance in both the low frequency range and the high frequency range can be obtained. If the diameter of the fiber mass 2 is appropriately selected, the second resin particles 4 can be easily dispersed and arranged in the second gaps 9, and the incidence of sound waves to the sound absorbing material 1 is not hindered, so that a sound absorbing material 1 having excellent sound absorbing performance in both the low frequency range and the high frequency range can be obtained.
[0087] Implementation method 4.
[0088] In this embodiment, an example in which the volume density of the sound absorbing material 1 is changed will be described. The other configurations are the same as those of the first embodiment. The sound absorbing performance is evaluated by the same method as that of the first embodiment.
[0089] <Example 8>
[0090] Set the bulk density to 48 kg / m 3 , and the sound absorbing material 1 was obtained in the same manner as in Example 1.
[0091] <Example 9>
[0092] Set the bulk density to 150 kg / m 3 , and the sound absorbing material 1 was obtained in the same manner as in Example 1.
[0093] <Example 10>
[0094] Set the bulk density to 190 kg / m 3, and the sound absorbing material 1 was obtained in the same manner as in Example 1.
[0095] The evaluation results are shown in Table 4. For reference, the evaluation results of Example 1 are shown again.
[0096] [Table 4]
[0097] Example 1 Example 8 Example 9 Example 10 <![CDATA[Volume density of filling material [kg / m 3 > 96 48 150 190 Frequency (500Hz) 1.96 1.90 2.02 1.98 Frequency (1000Hz) 1.15 1.10 1.17 1.07
[0098] The sound absorption coefficients of Example 1 and Example 8 to Example 10 are converted into coordinates. Figure 7 It can be seen that even if the volume density of the sound absorbing material 1 is changed, it still has excellent sound absorption rate. Figure 7 The dotted line in is an auxiliary line showing the behavior of the relative value of the sound absorption coefficient with respect to each volume density.
[0099] At 500 Hz, which is a low frequency range, the volume density of the sound absorbing material 1 is 48 kg / m 3 Example 8, bulk density 150kg / m 3 Example 9 and a bulk density of 190 kg / m 3 The relative values of the sound absorption rate of Example 10 are 1.90, 2.02, and 1.98, respectively, which are improved compared to 1 of Comparative Example 2. In addition, at 1000 Hz, which is a high frequency range, the relative values of the sound absorption rates of Examples 8, 9, and 10 are 1.10, 1.17, and 1.07, respectively, which are improved compared to 1 of Comparative Example 2. This shows that even if the volume density of the sound absorbing material 1 is changed, at 190 kg / m 3 The following will not reduce the sound absorption rate in the high-frequency range.
[0100] When the volume density of the sound absorbing material 1 is too high, the filler including the fiber mass 2, the first resin particles 3, and the second resin particles 4 is densely filled, which may hinder the incidence of sound waves on the sound absorbing material 1. If the volume density is too low, the filler is sparsely filled in the sound absorbing material 1, so the sound waves incident on the sound absorbing material 1 do not reach the first resin particles 3 and the second resin particles 4 and are emitted from the sound absorbing material 1, which may lead to low efficiency. Therefore, the volume density is preferably 30 kg / m 3 Above and 200kg / m 3 Below, more preferably 40kg / m 3 Above and 190kg / m 3 the following.
[0101] In this way, even if the volume density of the sound absorbing material 1 is changed, a sound absorbing material 1 having excellent sound absorbing performance in both the low frequency range and the high frequency range can be obtained. If the volume density is appropriately selected, the sound absorbing material 1 can absorb sound efficiently without hindering the incidence of sound waves to the sound absorbing material 1, so that a sound absorbing material 1 having excellent sound absorbing performance in both the low frequency range and the high frequency range can be obtained.
[0102] Implementation method 5.
[0103] In this embodiment, an example in which the first resin particles 3 and the magnetic particles 7 are captured in the first gaps 8 of the sound absorbing material 1 will be described. The other configurations are the same as those of the first embodiment.
[0104] like Figure 8 As shown, the first resin particles 3 and the magnetic particles 7 are captured in the first gaps 8 of the sound absorbing material 1 to form fiber clumps 2. Such a sound absorbing material 1 can recover the fiber clumps 2 by applying magnetic force from the outside. In addition, in particular, when the sizes of the plurality of fiber clumps 2 are different, they can be sorted by size.
[0105] Sorting using magnetic force, for example, can utilize the relationship between weight and magnetic force according to the size of the fiber block 2 in a magnetic sorting device. If the fiber block 2 becomes larger than the desired size, the fiber block 2 becomes heavier, and it is difficult to move the fiber block 2 by the attractive force or repulsive force generated by the external magnetic force. On the other hand, if the fiber block 2 becomes smaller than the desired size, the fiber block 2 becomes lighter, and it is easy to move the fiber block 2 by the attractive force or repulsive force generated by the external magnetic force. For example, if the recovery destination of the fiber block 2 is different according to the amount of movement of the fiber block 2, a fiber block 2 of the desired size with the magnetic particles 7 captured can be obtained. Among them, in the manufacturing process of the sound absorbing material 1, the magnetic particles 7 can be captured in the block formed by the fibers 6 entangled with each other before capturing the first resin particles 3, and the block can be magnetically sorted. In this way, blocks of different sizes can be sorted by size.
[0106] The magnetic particles 7 can be selected from one or more magnetic powder materials such as metal materials such as iron, ferrosilicon, nickel, Permalloy, Fe-Si-Al, Sendust, aluminum nickel cobalt magnet, samarium cobalt magnet, neodymium iron boron magnet, and ceramic materials such as spinel ferrite, hexagonal ferrite, garnet ferrite.
[0107] The particle size of the magnetic particles 7 is a particle size sufficient to obtain the desired magnetic force, and similarly to the first resin particles 3, it is sufficient to be captured in the first voids 8. For example, when the wire diameter of the fiber 6 is 7 μm, it can be greater than 0.05 mm and less than 1 mm, preferably greater than 0.1 mm and less than 0.5 mm.
[0108] Here, an example of a method for manufacturing a sound-absorbing material 1 using magnetic force is described. First, a mixture is prepared by mixing resin particles of different particle sizes such as polyurethane resin, a mass formed by entanglement of fibers 6, and magnetic particles 7 having a diameter that can be captured by the gaps formed in the mass (mixture preparation process). Next, the mixture is vibrated to capture small-diameter resin particles and magnetic particles 7 in the mass to produce a magnetic mass (magnetic mass preparation process). Next, the magnetic mass is recovered by magnetic force from the outside of the magnetic mass (magnetic mass recovery process). Furthermore, the unrecovered mixture is sieved to remove small-diameter resin particles that are not captured, and the minimum particle size of the resin particles remaining on the sieve is set as a threshold value, and large-diameter resin particles having a particle size above the threshold value are recovered (large-diameter particle recovery process). The composite of the mass and the large-diameter resin particles is filled in the package 5, and the large-diameter resin particles are dispersed in the package 5 to produce the sound-absorbing material 1 (composite filling process).
[0109] In this way, the small-diameter resin particles that become the first resin particles 3 are captured in the mass to form the fiber mass 2, and the fiber mass 2 is recovered by magnetic force, and the separated large-diameter resin particles are compounded as the second resin particles 4. When the composite is formed, the fibers 6 are entangled with each other to form a mass, and the sound absorbing material 1 having the fiber mass 2 having the first resin particles 3 captured in the first gaps 8 inside the mass and the second resin particles 4 having a particle size larger than the particle size of the first resin particles 3 and arranged in the second gaps 9 formed between the plurality of fiber mass 2 can be manufactured. Furthermore, by changing the magnetic force, the mass in which the small-diameter resin particles and the magnetic particles 7 are captured is recovered, so that the size of the fiber mass 2 can be easily made uniform, and the sound absorbing material 1 can be manufactured using the second resin particles 4 of a desired size, so that stable sound absorbing performance with small deviation can be obtained.
[0110] In addition, for example, a part or all of recycled products of air conditioners, refrigerators, etc. can be used as a material for constituting the sound absorbing material 1. An example of a method of producing the sound absorbing material 1 by recycling refrigerators will be described.
[0111] First, for example, an unwanted refrigerator is disassembled, and the housing of the heat-insulating body including a block formed by entanglement of resin such as polyurethane resin, magnetic material such as iron, and fibers 6 such as glass wool, and various components such as a compressor and a door seal are separated (separation process). Next, resin particles and magnetic particles 7 of different particle sizes and blocks contained in the heat-insulating body are recovered from the crushed powder obtained by crushing the housing and using wind power, magnetic force, etc. After recovery, the resin particles and magnetic particles 7 of different particle sizes can be further crushed to a desired size. In addition, small-diameter resin particles and magnetic particles 7 can be included in the block. Moreover, using the blocks formed by entanglement of fibers 6 obtained by recovery, resin particles of different particle sizes, and magnetic particles 7 having a diameter that can be captured by the gaps formed in the blocks, as shown in the example of the above-mentioned manufacturing method, through the mixture preparation process, magnetic block preparation process, magnetic block recovery process, large-diameter particle recovery process and composite filling process, the sound-absorbing material 1 can be manufactured from the recovered products.
[0112] Among them, for the recovered products, it is preferred to adopt a process of appropriately deodorizing, cleaning, etc. and then recovering, and to perform cleaning, impurity removal, etc. In addition, after the shell is crushed, the crushed powder is vibrated, and a plurality of magnetic blocks containing small-diameter resin particles and magnetic particles 7 in the blocks and a composite containing large-diameter resin particles are recovered, and the plurality of composites are filled in the packaging 5, and the large-diameter resin particles are dispersedly arranged in the packaging 5, so that the sound absorbing material 1 can be prepared. In this case, the sound absorbing performance of the manufactured sound absorbing material 1 can be checked, and the sound absorbing material 1 having the desired sound absorbing performance can be selected.
[0113] The sound absorbing material 1 manufactured in this way can effectively utilize resources and obtain a sound absorbing material 1 having excellent sound absorbing performance in both low-frequency range and high-frequency range. Furthermore, when the sound absorbing material 1 of the present invention having magnetic particles 7 is recycled, since the recycled products contain magnetic particles, the classification process can be made easier.
[0114] In the first to fifth embodiments, the same type of material may be selected for the first resin particles 3 and the second resin particles 4. For example, if a polyurethane resin is selected, a sound absorbing material 1 having excellent sound absorbing performance in both the low-frequency range and the high-frequency range can be obtained. Furthermore, it is more preferable that the number of material types of the sound absorbing material 1 is reduced, thereby stabilizing the durability, simplifying the manufacturing process, and facilitating the effective utilization of resources in recycling.
[0115] Furthermore, if the fibers 6 are given hydrophobicity, it is possible to prevent moisture from being present in the second gaps 9 between a plurality of blocks formed by the entanglement of the fibers 6 and in the first gaps 8 inside the blocks due to the mixing of moisture into the sound absorbing material 1 during the manufacture of the sound absorbing material 1, and it is more preferable because the second resin particles 4 can be easily arranged in the second gaps 9 and the first resin particles 3 can be easily captured in the first gaps 8. In this case, the fibers 6 or a block formed by the entanglement of the fibers 6 can be given hydrophobicity in part or in its entirety.
[0116] Furthermore, by having hydrophobicity, when water adheres to the fibers 6 due to condensation or the like after the manufacture of the sound absorbing material 1, it is possible to suppress the volume change of the first gap 8 caused by the reduction in the volume of the fiber mass 2 due to wetting of the fibers 6, and the reduction in the sound absorption performance of the sound absorbing material 1 due to the reflection of sound waves, etc. For the hydrophobic treatment, the fibers 6, the mass formed by the fibers 6 being entangled with each other, or the fiber mass 2 can be immersed in a hydrophobic material having water repellency such as mineral oil, synthetic oil, fluororesin, epoxy resin, silicone resin, etc. The hydrophobic material can also be sprayed to impart hydrophobicity to at least a portion of the mass formed by the fibers 6, the fibers 6 being entangled with each other, or the fiber mass 2. In this way, a better sound absorbing material 1 having excellent sound absorption performance in both the low frequency range and the high frequency range can be obtained.
[0117] In addition, the sound absorbing material 1 can be directly filled in the noise part according to the application instead of being filled in the packaging material 5. For example, for the noise of the outdoor unit of the air conditioner, it can be filled between the noise source such as the compressor and the air supply motor and the housing, and for the noise associated with the operation of the engine of the car, a part or all of the engine can be covered and fixed.
[0118] In addition to the above, the embodiments may be freely combined, any components of the embodiments may be modified, or any components of the embodiments may be omitted.
[0119] Description of Reference Numerals
[0120] 1 sound absorbing material, 2 fiber block, 3 first resin particles, 4 second resin particles, 5 packaging material, 6 fibers, 7 magnetic particles, 8 first gaps, 9 second gaps.
Claims
1. A sound absorbing material, comprising: Fiber block, wherein One or more fibers are entangled with each other to form a block, wherein the block has a first void inside and a first resin particle captured in the first void; and The second resin particles are arranged in the second gaps formed between the plurality of fiber blocks and have a particle size larger than that of the first resin particles.
2. The sound absorbing material according to claim 1, characterized in that: The second resin particles are selected from one or more of polyurethane resin, phenolic resin, epoxy resin, acrylic resin, polyester resin, polyamide resin, and melamine resin.
3. The sound absorbing material according to claim 1 or 2, characterized in that: The first resin particles are selected from one or more of polyurethane resin, phenolic resin, epoxy resin, acrylic resin, polyester resin, polyamide resin, and melamine resin.
4. The sound absorbing material according to any one of claims 1 to 3, characterized in that: The ratio of the particle diameter of the second resin particles to the particle diameter of the first resin particles is 2 or more.
5. The sound absorbing material according to any one of claims 1 to 4, characterized in that: The particle diameter of the second resin particles is 1 mm or more.
6. The sound absorbing material according to any one of claims 1 to 5, characterized in that: The diameter of the fiber mass is 5 mm or more and 70 mm or less.
7. The sound absorbing material according to any one of claims 1 to 6, characterized in that: The fiber has a linear diameter of 0.1 μm or more and 10 μm or less.
8. The sound absorbing material according to any one of claims 1 to 7, characterized in that: The bulk density of the filler material combined with the fiber block and the second resin particles is 30 kg / m 3 Above and 200kg / m 3 the following.
9. The sound absorbing material according to any one of claims 1 to 8, characterized in that: The fiber mass and the second resin particles are filled in a package.
10. The sound absorbing material according to any one of claims 1 to 9, characterized in that: Magnetic particles are captured in the first gaps of the fiber block.
11. The sound absorbing material according to any one of claims 1 to 10, characterized in that: At least a portion of the fibers, the blocks, or the fiber blocks is hydrophobic.
12. A method for manufacturing a sound absorbing material, comprising: a mixture preparation step, in which resin particles having different particle sizes, blocks formed by entanglement of fibers, and magnetic particles are mixed to prepare a mixture; a magnetic block manufacturing step, wherein the mixture is vibrated to capture the resin particles with small diameters and the magnetic particles among the resin particles with different particle diameters in the block to manufacture the magnetic block; a magnetic block recovery step, wherein the magnetic block is recovered by magnetic force; a large-diameter particle recovery step, wherein the unrecovered mixture is sieved to recover large-diameter resin particles having a particle size greater than a threshold value; and The composite filling step includes filling a composite formed by combining the magnetic block and the large-diameter resin particles into a package, and disposing the large-diameter resin particles in a dispersed manner in the package.
13. The method for manufacturing a sound absorbing material according to claim 12, characterized in that: Also included is a separation step, wherein the recovered product having a shell including a heat insulator is decomposed to separate the shell; The blocks formed by the fibers being entangled with each other are generated from the fibers contained in the insulator recovered by crushing the shell, the resin particles with different particle sizes are generated from the resin recovered by crushing the shell, and the magnetic particles are generated from the magnetic material recovered by crushing the shell.