Preparation of amidoximated MXene porous fiber membrane adsorption material imitating the structure of "rice paper" and uranium extraction method
Through the amidoximated MXene porous fiber membrane adsorption material imitating the "rice paper" structure, the siphon principle is used to optimize mass transfer in water, solving the problems of heat dissipation and low mass transfer efficiency in uranium extraction from seawater, and achieving low energy consumption and high efficiency. Excellent uranium adsorption performance, suitable for uranium extraction from seawater and other applications in complex environments.
Patent Information
- Application Number
- CN202310117131.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-15
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-02-15
AI Technical Summary
In the existing methods of extracting uranium from seawater, the heat dissipation of the adsorbent material is too large when it is in the water, which affects the adsorption performance, and the mass transfer efficiency is low, resulting in high energy consumption and expensive material costs, making it difficult to put into practical applications.
The amidoximated MXene porous fiber membrane adsorption material imitating the "rice paper" structure is used. The fiber has a porous structure through optimizing the preparation process. The siphon principle is used to optimize the mass transfer mode of water, reduce heat dissipation, and improve the adsorption sites and mass transfer rate. , to avoid additional energy consumption.
It achieves low energy consumption and efficient uranium adsorption performance, reduces heat conduction at the interface, increases the mass transfer rate within the water surface, expands the scope of application, reduces material costs, and is suitable for uranium extraction from seawater and other applications in complex environments.
Smart Images

Figure CN116440862B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing an adsorption material in the field of material preparation and uranium extraction from seawater, and in particular to a method for preparing an amidoximated MXene porous fiber membrane adsorption material with a "rice paper"-like structure and a method for extracting uranium. Background Art
[0002] At present, the main methods for extracting uranium from seawater are roughly divided into: membrane filtration, solvent extraction, ion exchange, adsorption, etc. Among them, the adsorption method is recognized as the most promising uranium extraction method due to its advantages of high efficiency, simple preparation, and low cost. Among the many adsorption materials, amidoxime-based materials have the greatest development potential due to their high affinity and ion selectivity for uranyl ions, acid and alkali resistance, and long service life.
[0003] The Chinese patent document with publication number CN113617341A discloses a double cross-linked hydrogel adsorbent for promoting uranium extraction from seawater by photothermal method and a preparation method thereof, comprising the following steps: adding a certain amount of polydopamine powder to an amidoxime polyacrylonitrile solution and stirring until dissolved, then adding sodium hydroxide to adjust the pH of the reaction solution to alkaline, and performing Michael addition reaction under light-proof conditions to obtain a PAO / PDA precursor solution; then adding ferric chloride solution and alkaline solution to adjust the pH to neutrality to perform cross-linking reaction to obtain a gel solution, and finally placing the solution in a mold for heating, forming, drying and washing to obtain a double cross-linked hydrogel adsorbent, wherein the mass ratio of amidoxime polyacrylonitrile to polydopamine is 0.2-0.6:1. The method of the present invention utilizes polydopamine to perform Michael addition reaction with amidoxime polyacrylonitrile and its reaction with Fe 3+ A double-crosslinked three-dimensional network structure hydrogel is prepared by a cross-linking reaction. The process is simple and the conditions are mild. The prepared adsorbent has high mechanical strength, good hydrophilicity, and has the advantage of promoting its ability to extract uranium from seawater through photothermal conversion performance.
[0004] The Chinese patent document with publication number CN114700044A discloses a method for preparing a photothermally enhanced antibacterial biomass / graphene aerogel uranium adsorbent, using graphene oxide, antibacterial biomass and amidoximated diaminomaleonitrile as raw materials, and preparing a photothermally enhanced antibacterial biomass / graphene aerogel uranium adsorbent through a one-step hydrothermal synthesis method. The uranium adsorbent prepared by the present invention has high mechanical strength, high photothermal conversion capacity and high antibacterial and antifouling properties, has unique and excellent adsorption properties for hexavalent uranium, good material stability, high reuse rate, and still has strong adsorption properties after 10 cycles of regeneration.
[0005] The Chinese patent document with publication number CN114931862A discloses a photothermal photocatalytic film for seawater desalination-uranium extraction and its preparation method, comprising the following steps: first, fix the treated carbon cloth on a glass plate, pour the casting liquid 1 on the carbon cloth to form a first film, then form the casting liquid 2 into a second film, and sequentially put it into the first coagulation bath and the second coagulation bath to form a photothermal photocatalytic film; the photothermal photocatalytic film is supported by the carbon cloth, and the surface has a micro-nano structure. The photothermal photocatalytic film prepared by the present invention can not only photocatalytically reduce uranium, but also separate and reduce uranium, and can separate and extract uranium while desalinating seawater; it can be used for seawater pretreatment to save costs.
[0006] The uranium adsorption materials that have been reported all use the photothermal effect of the material to improve the uranium adsorption performance. However, the above methods have the problem of excessive heat dissipation. When the material is placed in water, most of the heat energy generated at the interface is transferred to the water body, resulting in the temperature increase at the interface being limited, which in turn affects the improvement of adsorption performance. In addition, the above methods all use traditional mass transfer methods, mainly mass transfer of water from the outside to the inside of the membrane, while the mass transfer of water within the surface is slow, which limits the mass transfer efficiency of the water body.
[0007] Moreover, the above methods must increase additional energy consumption to achieve the improvement of mass transfer efficiency. The adsorption materials prepared by these methods have high energy consumption and complex reactions during the preparation process, and the raw materials used are expensive, making them difficult to be put into practical applications. Summary of the invention
[0008] In order to solve the problems existing in the background technology, the present invention provides an amidoxime-based MXene porous fiber membrane adsorption material, a preparation method and a method for extracting uranium from seawater, which has simple steps, a wide range of applications, excellent uranium adsorption performance and solves the problem of excessive heat dissipation.
[0009] The preparation method of the invention has simple steps, a wide range of applications, and requires abundant raw materials with a wide range of sources.
[0010] This invention optimizes the preparation process for the first time to make the fiber porous, greatly increase the adsorption sites and the in-plane mass transfer rate of the water body, and optimize the mass transfer mode of the water body by siphoning, which solves the problem of serious heat dissipation in the adsorption process while avoiding extra energy consumption. It has shown excellent performance in uranium adsorption and has great application prospects in various fields.
[0011] The technical solution adopted by the present invention is as follows:
[0012] (1) dissolving the raw materials in a main solvent at 60 to 70° C. for 0.5 to 5 hours, cooling to room temperature, adding anhydrous ethanol, and blending for 0.5 to 3 hours to obtain a blended solution;
[0013] (2) adding the photothermal material MXene to the blended solution obtained in (1) at 10 to 30° C. and stirring for 1 to 5 hours to obtain a MXene-modified polyamidooxime electrospinning solution as an amidoxime-based spinning solution;
[0014] (3) electrospinning the polyamidooxime electrospinning solution obtained in (2) under certain conditions, followed by freeze-drying for 24 to 72 hours to obtain a fiber membrane;
[0015] (4) The hydrophobic agent is then coated on the bottom surface of the fiber membrane for hydrophobic modification, thereby obtaining a porous fiber membrane with one side being hydrophobic and the other side being hydrophilic, which is used as an amidoxime-modified MXene porous fiber membrane adsorption material.
[0016] The raw materials involved in the step (1) are at least one of high molecular polymers such as polyamidoxime PAO, polyacrylonitrile PAN, polylactic acid PLA, polymethyl methacrylate PMMA, and polystyrene PS.
[0017] The main solvent involved in the step (1) is at least one of organic solvents such as N,N-dimethylformamide DMF, dimethyl sulfoxide DMSO, N,N-dimethylacetamide DMAC, N,N-diethylformamide DEF, N-methylpyrrolidone NMP, acetylacetone, and tetrachloroethylene.
[0018] The photothermal material involved in step (2) is at least one of black materials such as carbon black, carbon nanotubes, graphene, melanin, nanogold, nanoaluminum, black titanium dioxide, and titanium trioxide.
[0019] The hydrophobic agent involved in step (3) is polyacrylate coating, SiO 2f At least one of / SiO2 composite coatings, polydopamine-boehmite based composite materials, L-CNC / SiO2 composite coatings, and EP+PDMS / SiO2 composite coatings.
[0020] The mass ratio of the raw materials to the polyamidoxime electrospinning solution is 7-11wt%, the mass ratio of the main solvent to the polyamidoxime electrospinning solution is 75-82wt%, the mass ratio of anhydrous ethanol to the polyamidoxime electrospinning solution is 8-16wt%, and the mass ratio of MXene to the polyamidoxime electrospinning solution is 0.2-2.4mg / g.
[0021] In the step (3), the voltage range of the electrospinning is 5 kV to 30 kV, and the distance between the electrospinning nozzle and the receiving plate is 15 to 35 cm.
[0022] The prepared amidoxime-modified MXene porous fiber membrane material can be cross-linked with other substances, or other functional groups or loaded polymers can be grafted onto its surface to optimize uranium extraction performance and diversify material functions.
[0023] The amidoximated MXene porous fiber membrane adsorption material prepared by the present invention includes a variety of application fields, including applications in various complex environments in addition to uranium extraction from seawater, such as industrial wastewater treatment, radioactive element separation, environmental governance, precious metal recovery, seawater desalination, etc.
[0024] The method is to lay the middle part of the amidoxime MXene porous fiber membrane described in claim 7 flat on the surface of the reaction table, and the two ends naturally droop to form a "bridge-like" structure; under light, one end of the amidoxime MXene porous fiber membrane is immersed in a uranyl ion solution, and the other end is immersed in pure water; the liquid levels at the two ends are set to have a height difference, that is, the liquid levels of the uranyl ion solution and pure water have a height difference; the siphon effect and the porous structure of the amidoxime MXene porous fiber membrane are utilized to allow water and uranyl ions to quickly transfer laterally in the fiber membrane, thereby realizing the adsorption of uranyl ions, and the adsorption of uranyl ions is carried out under simulated sunlight.
[0025] In step (4), the illumination of simulated sunlight is set to have an illumination intensity ranging from 0.1 to 1.2 kW / m 2 .
[0026] In the step (4), the liquid level of the uranyl ion solution is higher than the liquid level of pure water, and the height difference of the liquid levels at both ends is adjusted to 3 to 9 cm.
[0027] The present invention is based on the reaction of PAO raw materials with DMF, and prepares polyamidoxi spinning solution by MXene modification, and then the spinning solution is allowed to enter an ethanol coagulation bath by an electrostatic spinning method to achieve phase separation, thereby forming porous fibers. It is then freeze-dried, and the resulting material is an amidoxime MXene porous fiber membrane adsorption material. By controlling the type, concentration and molecular weight of the raw materials for preparing the spinning solution, the light intensity, the spinning equipment parameters and the spinning conditions, the adsorption performance of the amidoxime-based MXene porous fiber membrane adsorption material is adjusted.
[0028] The present invention has the following advantages and beneficial effects:
[0029] The method of the present invention has simple steps, low energy consumption, and requires abundant raw materials, wide sources, and low cost. The prepared amidoxime-based MXene porous fiber membrane material can quickly generate heat by photothermal conversion, so that the fiber temperature inside the adsorption membrane rises rapidly, thereby improving the uranium adsorption capacity and adsorption specificity of the material for uranium. The porous fiber structure not only increases the adsorption sites of the fiber membrane, but also optimizes the mass transfer rate of water in the surface.
[0030] In addition, the present invention utilizes the siphon principle to achieve the purpose of controlling the water mass transfer rate by changing the height position of the liquid level at both ends of the membrane. The height difference generated by the siphon device and the introduction of the hydrophobic coating perfectly solve the problem of serious heat dissipation in the adsorption process. At the same time, the spontaneous siphon effect and the rapid mass transfer within the surface avoid the additional energy consumption generated to increase the mass transfer rate. Provide a new preparation method for the preparation field of amidoximation modified adsorption materials.
[0031] The membrane adsorption material prepared by the method of the present invention exhibits excellent performance in uranium adsorption and has great application prospects in the fields of uranium extraction from seawater, industrial wastewater treatment, radioactive element separation, environmental governance, precious metal recovery, seawater desalination, etc.
[0032] The advantages of the present invention are:
[0033] (1) For other adsorption materials, stirring and other methods are usually used to improve mass transfer efficiency, but the cost is increased energy consumption. The present invention uses the siphon effect to achieve spontaneous and rapid in-plane water mass transfer by selecting a suitable liquid level height difference without additional energy consumption;
[0034] (2) When the material is placed in water, most of the heat energy generated at the interface is conducted to the water body, resulting in a limited increase in temperature at the interface. The height difference generated by the siphon device of the present invention keeps most of the material away from the main aqueous solution, greatly reducing the heat conduction from the interface to the water body. At the same time, the introduction of the hydrophobic layer at the bottom of the material greatly reduces the thickness of the hydrophilic layer of the material. When water is transmitted to the plane at the solar radiation interface, the bottom hydrophobic layer can effectively prevent water from seeping down due to gravity and dripping from the material, thereby causing heat dissipation loss. In addition, the ultra-thin hydrophilic layer structure reduces in-plane heat convection and reduces heat dissipation.
[0035] (3) The present invention optimizes the preparation process to make the single fiber present a porous structure, further increasing the specific surface area of the material, increasing the uranium adsorption sites, and improving the uranium adsorption efficiency.
[0036] (4) In addition, compared with conventional fiber membranes, fiber membranes composed of single fibers with a porous structure are more hydrophilic and have a faster rate of water mass transfer within the surface, which changes the traditional mass transfer method that mainly transfers water from the outside to the inside of the membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 Diagram of the device for extracting uranium from seawater;
[0038] Figure 2The figure shows the adsorption performance of uranium by porous fiber membranes prepared with different raw materials, wherein the raw materials include: polylactic acid (PLA), polymethyl methacrylate (PMMA), polystyrene (PS), polyacrylonitrile (PAN), polyamidoximate (PAO);
[0039] Figure 3 This is a graph showing the adsorption performance of uranium on porous fiber membranes modified with different black substances;
[0040] Figure 4 The figure shows the adsorption performance of uranium by porous fiber membranes prepared with different mass percentages of PAO;
[0041] Figure 5 The figure shows the adsorption performance of uranium by porous fiber membranes prepared with different mass percentages of ethanol;
[0042] Figure 6 The adsorption performance of uranium on porous fiber membranes prepared using different concentrations of MXene;
[0043] Figure 7 This is a graph showing the adsorption performance of uranium at different light intensities;
[0044] Figure 8 The figure shows the adsorption performance of uranium on porous fiber membranes prepared using different spinning voltages;
[0045] Fig. 9 This is a graph showing the adsorption performance of uranium due to the different height differences of the liquid levels at both ends of the siphon device. DETAILED DESCRIPTION
[0046] The present invention is described in more detail by the following examples, but the examples are not intended to limit the present invention.
[0047] Embodiments of the present invention are as follows:
[0048] Example 1
[0049] PAO was selected as the raw material required for the reaction. At a temperature of 65°C, 9wt% PAO raw material was dissolved in 79wt% DMF solution for reaction for 3 hours, then cooled to room temperature, and anhydrous ethanol was added for blending for 1 hour; at 10-30°C, MXene was added and stirred for 2 hours to obtain an amidoxime-based electrospinning solution; then the obtained spinning solution was used for electrospinning, the spinning voltage was 15kV, the distance between the nozzle and the receiving plate was 16cm, and the temperature and humidity were 25°C and 40rh% respectively; the obtained porous fiber membrane was freeze-dried for 48 hours to obtain a dry amidoxime MXene porous fiber membrane. Then, a polyacrylate hydrophobic coating was used to hydrophobically modify the bottom surface of the fiber membrane to obtain a porous fiber membrane with one side hydrophobic and the other side hydrophilic.
[0050] The amidoxime-treated MXene porous fiber membrane was laid flat on the surface of the reaction table and naturally drooped to form a "bridge-like" structure. One end of the amidoxime-treated MXene porous fiber membrane was immersed in a uranyl ion solution with a concentration of 16ppm, pH=6, and a volume of 2L, and the other end was immersed in pure water. The height difference between the two ends of the liquid level was adjusted to 6cm, and a light intensity of 1.2kW / m was projected directly above the reaction table. 2 After 12 hours of adsorption, the content of uranyl ions in the solution was tested by ICP-MS. According to the test and analysis, the adsorption amount of uranyl ions by amidoxime MXene porous fiber membrane was 1637.65 mg / g.
[0051] Embodiments 2 to 5
[0052] Polyacrylonitrile (PAN), polylactic acid (PLA), polymethyl methacrylate (PMMA), polystyrene (PS) and other high molecular polymers were selected as raw materials, and the other conditions were the same as those in Example 1.
[0053] The results are shown in the following table and Figure 2 .
[0054] test Raw material type Uranium adsorption (mg / g) Example 2 Polylactic acid 621.20 Example 3 Polymethyl methacrylate 863.68 Example 4 Polystyrene 1028.68 Example 5 Polyacrylonitrile 1330.20
[0055] The results showed that the porous fiber membrane made by electrospinning with PAO as the raw material had the best adsorption performance (see Figure 2 ).
[0056] Embodiments 6 to 13
[0057] Carbon black, carbon nanotubes, graphene, melanin, nano-gold, nano-aluminum, black titanium dioxide, titanium trioxide and other black substances were selected as modified substances, and the other conditions were the same as those in Example 1. The results are shown in the following table and Figure 3 .
[0058]
[0059]
[0060] The results show that the amidoximated MXene porous fiber membrane with MXene as the black body has the best adsorption performance (see Figure 3 ).
[0061] Embodiments 14 to 17
[0062] The mass percentages of PAO were 7wt%, 8wt%, 10wt% and 11wt% respectively, and the other conditions were the same as those in Example 1. The results are shown in the following table and Figure 4 .
[0063] test PAO mass percentage Uranium adsorption performance (mg / g) Embodiment 14 7wt% 998.76 Embodiment 15 8wt% 1203.23 Example 16 10wt% 1576.34 Embodiment 17 11wt% 1339.71
[0064] The results show that the adsorption performance is best when the mass percentage of PAO is 9wt% (see Figure 4 ).
[0065] Examples 18 to 21
[0066] The mass percentages of ethanol were 8wt%, 10wt%, 14wt%, and 16wt%, respectively, and the other conditions were the same as in Example 1. The results are shown in the following table and Figure 5 .
[0067] test Ethanol mass percentage Uranium adsorption performance (mg / g) Embodiment 18 8wt% 1008.36 Embodiment 19 10wt% 1308.27 Embodiment 20 14wt% 1103.34 Embodiment 21 16wt% 919.71
[0068] The results showed that the adsorption performance was best when the ethanol mass percentage was 12wt% (see Figure 5 ).
[0069] Embodiments 22 to 25
[0070] The MXene concentrations were 0.2 mg / g, 0.8 mg / g, 1.6 mg / g, and 2.4 mg / g, respectively, and the other conditions were the same as in Example 1. The results are shown in the following table and Figure 6 .
[0071]
[0072]
[0073] The results show that the adsorption performance is best when the MXene concentration is 2.0 mg / g (see Figure 6 ).
[0074] Embodiments 26 to 29
[0075] Adjust the light intensity to 0.1kW / m 2 , 0.2kW / m 2 , 0.4kW / m 2 , 0.8kW / m 2 , and the other conditions are the same as in Example 1. The results are shown in the following table and Figure 7 .
[0076]
[0077] The results show that the light intensity is 1.2kW / m 2 When , the adsorption performance is the best. (See Figure 7 )
[0078] Embodiments 30 to 33
[0079] The spinning voltage of the electrospinning machine was adjusted to 5 kV, 10 kV, 20 kV, and 25 kV respectively, and the other conditions were the same as in Example 1. The results are shown in the following table and Figure 8 .
[0080]
[0081] The results show that the adsorption performance is best when the spinning voltage is 15kV. Figure 8 )
[0082] Embodiments 34 to 37
[0083] The height difference of the liquid level at both ends of the siphon device was adjusted to 3.0 cm, 4.5 cm, 7.5 cm, and 9.0 cm respectively, and the other conditions were the same as in Example 1. The results are shown in the following table and Fig. 9 .
[0084]
[0085] The results show that the adsorption performance is best when the liquid level difference is 6.0 cm (see Fig. 9 ).
Claims
1. A method for preparing an amidoximated MXene porous fiber membrane adsorption material with a "rice paper" structure, characterized in that: The method comprises the following steps: (1) Dissolve the raw materials in the main solvent at 60-70 °C for 0.5-5 hours, cool to room temperature, add anhydrous ethanol, and mix for 0.5-3 hours to obtain a blended solution; The raw material involved in step (1) is polyamidoximate PAO; The main solvent involved in step (1) is at least one of N,N-dimethylformamide DMF, dimethyl sulfoxide DMSO, N,N-dimethylacetamide DMAC, N,N-diethylformamide DEF, N-methylpyrrolidone NMP, acetylacetone, and tetrachloroethylene organic solvents; (2) adding the photothermal material MXene to the blended solution obtained in step (1) at 10-30°C, stirring for 1-5 hours, and obtaining a MXene-modified polyamidoximine electrospinning solution; The mass ratio of the raw materials to the MXene-modified polyamidoxime electrospinning solution is 7-11 wt %, the mass ratio of the main solvent to the MXene-modified polyamidoxime electrospinning solution is 75-82 wt %, the mass ratio of anhydrous ethanol to the MXene-modified polyamidoxime electrospinning solution is 8-16 wt %, and the mass ratio of the MXene to the MXene-modified polyamidoxime electrospinning solution is 0.2-2.4 mg / g; (3) electrospinning the MXene-modified polyamidoximine electrospinning solution obtained in step (2) under certain conditions, and then freeze-drying it for 24 to 72 hours to obtain a fiber membrane; (4) A hydrophobic agent is then coated on the bottom surface of the fiber membrane for hydrophobic modification, thereby obtaining a porous fiber membrane with one side being hydrophobic and the other side being hydrophilic, which serves as an amidoxime-modified MXene porous fiber membrane.
2. The preparation method according to claim 1, characterized in that: The hydrophobic agent involved in step (4) is polyacrylate coating, SiO 2f At least one of / SiO2 composite coatings, polydopamine-boehmite based composite materials, L-CNC / SiO2 composite coatings, and EP+PDMS / SiO2 composite coatings.
3. The preparation method according to claim 1, characterized in that: In the step (3), the voltage range of the electrospinning is 5 kV to 30 kV, and the distance between the electrospinning nozzle and the receiving plate is 15 to 35 cm.
4. A MXene porous fiber membrane adsorption material with amidoximation structure imitating "rice paper", characterized in that: The amidoximated MXene porous fiber membrane adsorption material is prepared by the preparation method described in any one of claims 1-3.
5. An application of the amidoximated MXene porous fiber membrane adsorption material according to claim 4, characterized in that: Used in uranium extraction from seawater.
6. A method for extracting uranium using the amidoximated MXene porous fiber membrane adsorption material according to claim 4, characterized in that: The method is to lay the middle part of the amidoxime MXene porous fiber membrane adsorption material described in claim 4 flat on the surface of the reaction table, and the two ends naturally droop to form a "bridge-like" structure, and immerse one end of the amidoxime MXene porous fiber membrane in a uranyl ion solution and the other end in pure water under light, and set the liquid levels at the two ends to have a height difference, and utilize the siphon effect and the porous structure of the amidoxime MXene porous fiber membrane to make water and uranyl ions transfer laterally in the fiber membrane, so as to achieve the adsorption of uranyl ions; The liquid level of the uranyl ion solution is higher than that of pure water, and the height difference of the liquid levels at both ends is adjusted to 3~9 cm.
7. The method for extracting uranium according to claim 6, characterized in that: Set the illumination to simulate sunlight, with the illumination intensity ranging from 0.1 to 1.2 kW / m 2 .
Citation Information
Patent Citations
Bi-crosslinking hydrogel adsorbent for promoting uranium extraction from seawater through photo-thermal and preparation method of bi-crosslinking hydrogel adsorbent
CN113617341A
Preparation method of photo-thermal enhanced antibacterial biomass / graphene aerogel uranium adsorbent
CN114700044A
A photothermal and photocatalytic membrane for seawater desalination and uranium extraction co-production and its preparation method
CN114931862A
Nanofiber membrane and membrane adsorbing assembly for extracting uranium from seawater and brine water and application of nanofiber membrane and membrane adsorbing assembly
CN105080509A
Preparation method of Mxene membrane adsorption material based on polyamidoxime and uranium extraction method
CN112973653A