A catalyst grading method and its application
Through multi-stage catalyst gradation, the coordination type of aluminum ions in the alumina carrier is adjusted, the pore structure and activity of the catalyst are optimized, the problem of mismatch between the molecular structure of the reactant and the microstructure of the catalyst in the existing technology is solved, and inferior raw materials are realized. Long-term stable operation and improved catalyst performance.
Patent Information
- Application Number
- CN202210012024.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-01-06
AI Technical Summary
Existing heavy oil hydrogenation catalyst grading methods fail to effectively match the molecular structure of the reactants and the microstructure of the catalyst, resulting in a limited depth of hydrogenation reaction and difficulty in achieving long-term stable operation of inferior raw materials.
A multi-stage catalyst gradation system is adopted, in which each stage of the catalyst contains an alumina carrier and three coordination types of aluminum ions. Five-coordinated, four-coordinated and three-coordinated aluminum are gradually adjusted along the flow direction of the liquid phase reactants. The content of ions can optimize the pore structure and activity of the catalyst and improve the utilization rate of the catalyst.
By optimizing the microstructure of the catalyst, the interaction between metal and alumina defects is enhanced, the deactivation of the catalyst is inhibited, the impurity removal efficiency is improved, the device operation cycle is extended, and the catalytic performance of the catalyst is improved.
Smart Images

Figure CN116440917B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a catalyst grading method and application thereof, in particular to a catalyst grading method for heavy oil hydrogenation catalyst for long-term operation of inferior raw materials and application thereof. Background Art
[0002] During the heavy oil hydrogenation process, as the raw materials become heavier and inferior, the content of metal impurities and inorganic salts such as Fe, Si, Na, Ca in the raw materials continues to increase. These metals mainly exist in the form of colloids and asphaltene. Secondly, the heavy inferior raw materials have low saturated hydrocarbon content, high aromatic hydrocarbon content, and high colloid content, especially high heavy aromatic hydrocarbon content. These heavy raw materials have complex molecular structures, large steric hindrance, and impurities are easier to remove; with the hydrogenation and hydrogenolysis reactions, the reactant molecules gradually open the ring and break the chain, the molecular structure is gradually simplified, the steric hindrance is small, and impurities are more difficult to remove. At present, the grading method of heavy oil hydrogenation catalyst is often studied from the surface level, that is, the catalyst particle size, pore size and activity transition, and it is not considered from the actual reactant molecular structure level and catalyst microstructure. As the reaction proceeds, the reactant molecular structure and catalyst microstructure cannot match well, which limits the depth of the hydrogenation reaction.
[0003] CN103773437A discloses a grading method for a hydrodesulfurization catalyst, the method comprising: a hydrogenation reactor includes at least two catalyst beds, in accordance with the order of contact with the reaction material, the upstream bed is a low-pile ratio catalyst bed, the downstream catalyst bed has a higher pile ratio than the adjacent upstream catalyst bed; each catalyst bed is graded and loaded with two or more catalysts of different diameters. These physical mixtures have a smaller void ratio and a larger loading pile ratio than their single diameter catalysts, which improves the hydrodesulfurization performance of the entire reaction system, but it is difficult to achieve long-term stable operation for processing inferior raw materials with high solid impurity content. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a catalyst grading method to solve the problem of long-term operation of inferior raw materials, to effectively optimize the activity grading of the overall catalyst, to achieve a reasonable distribution of impurities in the entire system, and thus to achieve the purpose of synchronous deactivation of the entire catalyst system as much as possible, so as to improve the utilization rate of the catalyst and achieve long-term operation of the device.
[0005] To achieve the above object, the present invention provides a catalyst grading method, comprising a grading system consisting of n-level catalysts, wherein n ≥ 3, preferably n is 3 or 4, each level of catalyst comprises an alumina carrier, and the alumina carrier contains three types of aluminum ions: tri-coordinated aluminum ions Al 3+ III , four-coordinated aluminum ion Al 3+IV and pentacoordinated aluminum ion Al 3+ V The n-level catalyst grading satisfies the following conditions: along the flow direction of the liquid phase reactant, based on the total amount of three ligands of aluminum in the alumina carrier, the content of penta-coordinated aluminum ions is It decreases gradually, with the decreasing range being 5 to 15 percentage points.
[0006] Furthermore, along the flow direction of the liquid phase reactants, the content of the tri-coordinated aluminum ion is based on the total amount of the three ligands of aluminum in the alumina carrier. The increase is gradual, with the increment ranging from 1 to 10 percentage points.
[0007] Furthermore, along the flow direction of the liquid phase reactants, based on the total amount of the three ligands of aluminum in the alumina carrier, the content of the tetracoordinated aluminum ion There are no specific requirements and it can be increased, decreased or unchanged.
[0008] Furthermore, in the alumina carrier of each catalyst stage, the content of penta-coordinated aluminum ions is based on the total content of the three ligand aluminums. The content of tetracoordinate aluminum ions is 40-60%. The content of tri-coordinated aluminum ions is 30% to 50%. It is 10% to 30%.
[0009] Furthermore, the contents of various types of coordinated aluminum ions are calculated as shown in formulas I, II, and III:
[0010]
[0011]
[0012]
[0013] where θ represents the molar number of coordinated aluminum ions, is the coordinated aluminum ion content.
[0014] Furthermore, in the alumina carrier of the same grade catalyst, the content of pentacoordinated aluminum ions is
[0015] Furthermore, in the alumina carrier of the same grade of catalyst, the difference between the content of penta-coordinated aluminum ions and the content of tri-coordinated aluminum ions is 15% to 50%.
[0016] Furthermore, the n is preferably 3, that is, the graded system contains three catalysts. Based on the total volume of the catalyst in the reactor, the three-stage filling ratios along the flow direction of the liquid reactants are 10% to 90%: 5% to 40%: 5% to 80%, and the sum of the filling ratios of each level is 100%.
[0017] Furthermore, the n is preferably 4, that is, the graded system contains four catalysts. Based on the total volume of the catalyst in the reactor, along the flow direction of the liquid reactants, the four-stage filling ratio is: 10% to 70%: 10% to 40%: 10% to 40%: 10% to 70%, and the sum of the filling ratios of each level is 100%; the preferred filling ratios are: 10% to 40%: 10% to 40%: 10% to 40%: 10% to 40%, and the sum of the filling ratios of each level is 100%.
[0018] Furthermore, the catalyst includes an active metal component.
[0019] Furthermore, the alumina carrier is prepared by molding / modifying hydrated alumina and / or an alumina composition; wherein the hydrated alumina and / or the alumina composition contains tri-coordinated aluminum ions, tetra-coordinated aluminum ions and penta-coordinated aluminum ions.
[0020] Furthermore, the catalyst is a hydrogenation catalyst, preferably an oxidized hydrogenation catalyst before sulfurization; further preferably, a heavy oil hydrogenation catalyst commonly used in the art, wherein, along the flow direction of the reactants, the pore volume of each hydrogenation catalyst decreases step by step, the pore size decreases step by step, the activity increases step by step, and the particle size decreases step by step, such as a hydrogenation protective agent, a hydrogenation demetallization agent, a hydrogenation desulfurization agent, a hydrogenation carbon removal agent, a hydrogenation denitrification agent, etc.
[0021] Furthermore, the catalyst uses Group VIII and / or Group VIB metal elements as active metal components, and based on the weight of the catalyst, the active metal is calculated as oxide, the Group VIII metal content is 0.2wt% to 9.0wt%, preferably 0.5wt% to 9.0wt%, and the Group VIB metal content is 4wt% to 50wt%, preferably 4wt% to 45wt%.
[0022] Furthermore, in the catalyst, based on the weight of the catalyst, the content of the alumina carrier is 45wt% to 95wt%, preferably 50wt% to 95wt%.
[0023] Furthermore, in the alumina carrier, the control of the content of different coordinated aluminum mainly depends on the calcination temperature during the preparation of the alumina carrier. Increasing the calcination temperature increases the content of penta-coordinate aluminum, while decreasing the calcination temperature increases the content of tri-coordinate aluminum.
[0024] Furthermore, the content of different coordinated aluminum in the alumina carrier can also be controlled by adjusting the pH value during the preparation process of the alumina carrier.
[0025] Furthermore, the calcination temperature during the preparation of the alumina carrier is 300-1000°C.
[0026] Furthermore, it is preferred that the catalyst grading system includes three-stage catalysts, and the three-stage catalysts all contain alumina carriers, namely: alumina carrier I, alumina carrier II and alumina carrier III, wherein the calcination temperature of alumina carrier I is preferably 700-1000°C, and the calcination time is 2-10h; the calcination temperature of alumina carrier II is preferably 500-700°C, and the calcination time is 2-10h; the calcination temperature of alumina carrier III is preferably 300-500°C, and the calcination time is 2-10h.
[0027] In the method of the present invention, the synthesis method of alumina used in the alumina carrier I refers to the reaction for preparing aluminum hydroxide gel, which can be specifically one or more of precipitation method (including acid method and alkali method), hydrolysis method, etc. The precipitation method can be one or more of aluminum sulfate method, carbonization method, aluminum chloride method, aluminum nitrate method, etc.; the hydrolysis method can be a hydrolysis reaction of aluminum-containing compounds, such as the hydrolysis of low-carbon aluminum alcohol and high-carbon aluminum alcohol. The prepared alumina raw material is kneaded and extruded into a plastic body, and finally dried and calcined to obtain the desired alumina carrier precursor, the drying temperature is 100-200°C, the calcination temperature is 700-1000°C, and the calcination time is 2-10h.
[0028] In the method of the present invention, the synthesis method of alumina used in the alumina carrier II refers to the reaction for preparing aluminum hydroxide gel, which can be specifically one or more of precipitation method (including acid method and alkali method), hydrolysis method, etc. The precipitation method can be one or more of aluminum sulfate method, carbonization method, aluminum chloride method, aluminum nitrate method, etc.; the hydrolysis method can be the hydrolysis reaction of aluminum-containing compounds, such as the hydrolysis of low-carbon aluminum alcohol and high-carbon aluminum alcohol. Then the prepared alumina raw material is kneaded and extruded into a plastic body, and finally dried and calcined to obtain the desired alumina carrier precursor, the drying temperature is 100-200°C, the calcination temperature is 500-700°C, and the calcination time is 2-10h.
[0029] In the method of the present invention, the synthesis method of alumina used in the alumina carrier III refers to the reaction for preparing aluminum hydroxide gel, which can be specifically one or more of precipitation method (including acid method and alkali method), hydrolysis method, etc. The precipitation method can be one or more of aluminum sulfate method, carbonization method, aluminum chloride method, aluminum nitrate method, etc.; the hydrolysis method can be the hydrolysis reaction of aluminum-containing compounds, such as the hydrolysis of low-carbon aluminum alcohol and high-carbon aluminum alcohol. The prepared alumina raw material is kneaded and extruded into a plastic body, and finally dried and calcined to obtain the desired alumina carrier precursor, the drying temperature is 100-200°C, the calcination temperature is 300-500°C, and the calcination time is 2-10h.
[0030] The second aspect of the present invention is to provide an application of the above catalyst grading method in the hydroprocessing of inferior raw materials.
[0031] Furthermore, the inferior raw materials include: heavy inferior raw materials such as gasoline, diesel, wax oil, residual oil, coal tar, coal liquefied oil, etc., especially residual oil.
[0032] In the method of the present invention, the catalyst in the graded system is preferably vulcanized before use, and the vulcanization method can be wet vulcanization or dry vulcanization.
[0033] Furthermore, the catalyst grading method of the present invention can be used under any hydroprocessing reaction conditions suitable in the art.
[0034] Furthermore, the hydroprocessing reaction conditions are as follows: the average reaction temperature is 200°C to 450°C, preferably 250°C to 430°C; the reaction hydrogen partial pressure is 4.0MPa to 20.0MPa, preferably 8.0MPa to 18.0MPa; the liquid hourly volume space velocity is 0.15h -1 ~3.0h -1 , preferably 0.2h -1 ~2.0h -1 ; The volume ratio of hydrogen to oil is 300 to 1500, preferably 500 to 1200.
[0035] Compared with the prior art, the method of the present invention has the following advantages:
[0036] In the method of the present invention, along the flow direction of the liquid phase reactant, the modified alumina carrier in the hydrogenation catalyst firstly used has a higher content of penta-coordinated aluminum ions, a moderate content of tetra-coordinated aluminum ions, and a lower content of tri-coordinated aluminum ions, thereby enhancing the interaction between the metal and the alumina defects and weakening the interaction between hydrogen and the alumina surface, thereby increasing the overflow of hydrogen on the catalyst surface. The overflow hydrogen can enhance the catalytic performance of the catalyst, inhibit the deactivation of the catalyst, enable the removal of more metals such as Ni, Fe, V, etc., and reduce the carbon on the surface; and the modified alumina carrier in the hydrogenation catalyst finally used has a lower content of penta-coordinated aluminum ions, a moderate content of tetra-coordinated aluminum ions, and an increased content of tri-coordinated aluminum ions, thereby weakening the interaction between the metal and the alumina defects, increasing the active sites, and reducing the steric hindrance of the reactants, thereby facilitating the removal of impurities such as O, S, N, etc. that are difficult to remove in small molecules. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The NMR analysis results of the alumina carrier I of the catalyst used in Example 1;
[0038] Figure 2 The NMR analysis results of the alumina carrier II of the catalyst used in Example 1;
[0039] Figure 3 This is the nuclear magnetic resonance analysis result of the alumina carrier III of the catalyst used in Example 1. DETAILED DESCRIPTION
[0040] The preparation method of the catalyst of the present invention is described in more detail below through specific examples. The examples are only illustrative of the specific implementation of the method of the present invention and do not constitute a limitation on the scope of protection of the present invention.
[0041] Unless otherwise specified in the present invention, the content of coordinated aluminum ions is molar content.
[0042] In the method of the present invention, the specific surface area and pore structure of the hydrogenation catalyst are measured by low-temperature nitrogen adsorption.
[0043] In the present invention, a Bruker AVANCE III 500 nuclear magnetic resonance spectrometer is used to determine the type and quantity of aluminum ions. Experimental conditions: BBO normal phase observation broadband probe, H decoupling, deuterium lock channel; standard broadband range: BB = 31P-15N; sensitivity: 367S / N1HNMR, 0.1EB 263S / N 13CNMR, ASTM; resolution: 0.38HZ1H, 0.1CHCL3, 0.13 13C NMR, ASTM.
[0044] Example 1
[0045] This embodiment provides a catalyst grading solution to solve the problem of long-term operation of inferior raw materials, that is, loading catalysts in the reactor, and loading hydrogenation catalyst I, hydrogenation catalyst II and hydrogenation catalyst III from top to bottom along the flow direction of liquid reactants in the bed, wherein the loading volume ratio of hydrogenation catalysts I, II and III is 50%:25%:25%.
[0046] The alumina used in the hydrogenation catalyst I is prepared by hydrolyzing aluminum isopropoxide, kneaded and extruded into a plastic body, dried at 120°C for 3 hours, and calcined at 900°C for 3 hours to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 55%, and the content of tetracoordinate aluminum ions Φ IV The value is 35%, and the content of tri-coordinated aluminum ions Φ III The value is 10%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 120℃ for 3h, and calcined at 500℃ for 3h to obtain hydrogenation catalyst I. The prepared catalyst I contains 6.5% MoO3, 0.7% NiO, and 92.8% alumina carrier; the properties of the catalyst are as follows: the specific surface area is 100m 2 / g, and the pore diameter is 17.8nm.
[0047] The alumina used in the hydrogenation catalyst II is prepared by the aluminum sulfate method. Urea is added during the kneading process to extrude into a plastic body, which is then dried at 120°C for 2 hours and calcined at 700°C for 3 hours to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II is Φ V The value is 45%, and the content of tetracoordinated aluminum ions Φ IV The value is 40%, and the content of tri-coordinated aluminum ions Φ III The value is 15%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 150℃ for 2h, and calcined at 450℃ for 4h to obtain hydrogenation catalyst II. The prepared catalyst II contains 12.0% MoO3, 2.5% NiO, and 85.5% alumina carrier; the properties of the catalyst are as follows: specific surface area is 175m 2 / g, and the pore diameter is 12.8nm.
[0048] The alumina used in the hydrogenation catalyst III is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 150°C for 2 hours and calcined at 500°C for 3 hours to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 40%, and the content of tetracoordinated aluminum ions is Φ IV The value is 35%, and the content of tri-coordinated aluminum ions Φ IIIThe value is 25%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 120℃ for 4h, and calcined at 480℃ for 3h to obtain hydrogenation catalyst III. The prepared catalyst III contains 21.5% MoO3, 3.6% NiO, and 74.9% alumina carrier; the properties of the catalyst are as follows: specific surface area is 190m 2 / g, and the pore diameter is 8.2nm.
[0049] Example 2
[0050] This embodiment provides a catalyst grading solution for long-term operation of inferior raw materials, that is, loading catalysts in the reactor, and loading hydrogenation catalyst I, hydrogenation catalyst II and hydrogenation catalyst III from top to bottom along the flow direction of liquid reactants in the bed, wherein the loading volume ratio of hydrogenation catalysts I, II and III is 50%:30%:20%.
[0051] The alumina used in the hydrogenation catalyst I is prepared by the aluminum sulfate method, and after being mixed and kneaded into a plastic body, it is dried at 150°C for 3 hours and calcined at 950°C for 4 hours to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 60%, and the content of tetracoordinated aluminum ions Φ IV The value is 30%, and the content of tri-coordinated aluminum ions Φ III The value is 10%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 150°C for 4h, and calcined at 480°C for 3h to obtain hydrogenation catalyst I. The prepared catalyst I contains 4.5% MoO3, 0.9% NiO, and 94.6% alumina carrier; the properties of the catalyst are as follows: the specific surface area is 110m 2 / g, and the pore diameter is 16.9nm.
[0052] The alumina used in the hydrogenation catalyst II is prepared by the alcohol aluminum method. After adding ethylenediamine during the kneading process, it is extruded into a plastic body, dried at 120°C for 2 hours, and calcined at 600°C for 3 hours to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II is Φ V The value is 50%, and the content of tetracoordinated aluminum ions Φ IV The value is 40%, and the content of tri-coordinated aluminum ions Φ III The value is 15%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 120℃ for 5h, and calcined at 470℃ for 4h to obtain hydrogenation catalyst II. The prepared catalyst II contains 12.2% MoO3, 2.7% NiO, and 85.1% alumina carrier; the properties of the catalyst are as follows: specific surface area is 179m 2 / g, and the pore diameter is 13.8nm.
[0053] The alumina used in the hydrogenation catalyst III is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 150°C for 2 hours and calcined at 450°C for 3 hours to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 45%, and the content of tetracoordinated aluminum ions Φ IV The value is 35%, and the content of tri-coordinated aluminum ions Φ III The value is 20%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 150℃ for 4h, and calcined at 450℃ for 3h to obtain hydrogenation catalyst III. The prepared catalyst III contains 22.5% MoO3, 3.9% NiO, and 73.6% alumina carrier; the properties of the catalyst are as follows: specific surface area is 200m 2 / g, and the pore diameter is 9.9nm.
[0054] Example 3
[0055] This embodiment provides a catalyst grading solution for long-term operation of inferior raw materials, that is, catalysts are loaded in the reactor, and the bed is loaded with hydrogenation catalyst I, hydrogenation catalyst II and hydrogenation catalyst III from top to bottom along the flow direction of the liquid reactants, wherein the filling volume ratio of hydrogenation catalysts I, II and III is 15%:25%:60%.
[0056] The alumina used in the hydrogenation catalyst I is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 200°C for 3 hours and calcined at 800°C for 3 hours to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 50%, and the content of tetracoordinated aluminum ions Φ IV The value is 40%, and the content of tri-coordinated aluminum ions Φ III The value is 10%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 150°C for 4h, and calcined at 490°C for 3.5h to obtain hydrogenation catalyst I. The prepared catalyst I contains 4.3% MoO3, 0.7% NiO, and 95% alumina carrier; the properties of the catalyst are as follows: the specific surface area is 101m 2 / g, and the pore diameter is 22.7nm.
[0057] The alumina used in the hydrogenation catalyst II is prepared by the aluminum sulfate method. After diethylene glycol is added during the kneading process to extrude into a plastic body, it is dried at 120°C for 2 hours and calcined at 700°C for 3 hours to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II is Φ V The value is 45%, and the content of tetracoordinated aluminum ions Φ IV The value is 40%, and the content of tri-coordinated aluminum ions ΦIII The value is 15%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 120℃ for 3h, and calcined at 500℃ for 3h to obtain hydrogenation catalyst II. The prepared catalyst II contains 12.3% MoO3, 1.9% NiO, and 85.8% alumina carrier; the properties of the catalyst are as follows: specific surface area is 156m 2 / g, and the pore diameter is 15.2nm.
[0058] The alumina used in the hydrogenation catalyst III is prepared by the alcohol aluminum method, and after being mixed and kneaded into a plastic body, it is dried at 150°C for 2 hours and calcined at 500°C for 3 hours to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 40%, and the content of tetracoordinated aluminum ions is Φ IV The value is 40%, and the content of tri-coordinated aluminum ions Φ III The value is 20%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 150℃ for 4h, and calcined at 500℃ for 4h to obtain hydrogenation catalyst III. The prepared catalyst III contains 20.3% MoO3, 3.6% NiO, and 76.1% alumina carrier; the properties of the catalyst are as follows: specific surface area is 231m 2 / g, and the pore diameter is 9.2nm.
[0059] Comparative Example 1
[0060] This example provides a catalyst grading solution for long-term operation with inferior raw materials, namely, loading catalysts in the reactor, and loading hydrogenation catalyst I, hydrogenation catalyst II and hydrogenation catalyst III from top to bottom along the flow direction of liquid reactants in the bed, wherein the loading volume ratio of hydrogenation catalysts I, II and III is 50%:25%:25%.
[0061] The modified alumina used in the hydrogenation catalyst I is prepared by hydrolyzing aluminum isopropoxide, and after being kneaded and extruded into a plastic body, it is dried at 150°C for 3 hours and calcined at 950°C for 4 hours to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 60%, and the content of tetracoordinated aluminum ions Φ IV The value is 30%, and the content of tri-coordinated aluminum ions Φ III The value is 10%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 120℃ for 5h, and calcined at 500℃ for 4h to obtain hydrogenation catalyst I. The prepared catalyst I contains 4.5% MoO3, 0.9% NiO, and 94.6% alumina carrier; the properties of the catalyst are as follows: specific surface area is 110m 2 / g, and the pore diameter is 16.9nm.
[0062] The modified alumina used in the hydrogenation catalyst II is prepared by hydrolyzing aluminum isopropoxide, and after being kneaded and extruded into a plastic body, it is dried at 150°C for 3 hours and calcined at 700°C for 4 hours to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 57%, and the content of tetracoordinate aluminum ions Φ IV The value is 33%, and the content of tri-coordinated aluminum ions Φ III The value is 10%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 140℃ for 2.5h, and calcined at 480℃ for 4h to obtain hydrogenation catalyst II. The prepared catalyst II contains 12.2% MoO3, 2.7% NiO, and 85.1% alumina carrier; the properties of the catalyst are as follows: specific surface area is 156m 2 / g, and the pore diameter is 13.8nm.
[0063] The modified alumina used in the hydrogenation catalyst III is prepared by hydrolyzing aluminum isopropoxide, and after being kneaded and extruded into a plastic body, it is dried at 150°C for 3 hours and calcined at 500°C for 4 hours to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared alumina carrier I is Φ V The value is 55%, and the content of tetracoordinate aluminum ions Φ IV The value is 33%, and the content of tri-coordinated aluminum ions Φ III The value is 12%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 160℃ for 3.5h, and calcined at 420℃ for 5h to obtain hydrogenation catalyst III. The prepared catalyst III contains 12.2% MoO3, 2.7% NiO, and 85.1% alumina carrier; the properties of the catalyst are as follows: specific surface area is 156m 2 / g, and the pore diameter is 13.8nm.
[0064] Comparative Example 2
[0065] This example provides a catalyst grading solution for long-term operation with inferior raw materials, namely, loading catalysts in the reactor, and loading hydrogenation catalyst I, hydrogenation catalyst II and hydrogenation catalyst III from top to bottom along the flow direction of the liquid reactants, wherein the loading volume ratio of hydrogenation catalysts I, II and III is 40%:25%:35%.
[0066] The modified alumina used in the hydrogenation catalyst I was prepared by the aluminum sulfate method. After diethylene glycol was added during the kneading process to extrude into a plastic body, it was dried at 120°C for 2 hours and calcined at 800°C for 3 hours to obtain the desired alumina carrier I. The content of pentacoordinated aluminum ions in the prepared alumina carrier I was Φ V The value is 45%, and the content of tetracoordinated aluminum ions ΦIV The value is 40%, and the content of tri-coordinated aluminum ions Φ III The value is 15%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 120℃ for 3h, and calcined at 500℃ for 3h to obtain hydrogenation catalyst I. The prepared catalyst I contains 6.5% MoO3, 0.7% NiO, and 92.8% alumina carrier; the properties of the catalyst are as follows: the specific surface area is 100m 2 / g, and the pore diameter is 17.8nm.
[0067] The modified alumina used in the hydrogenation catalyst II was prepared by the aluminum sulfate method. After adding diethylene glycol during the kneading process, it was extruded into a plastic body, dried at 120°C for 2h, and calcined at 700°C for 3h to obtain the desired alumina carrier II. The content of pentacoordinated aluminum ions in the prepared alumina carrier II was Φ V The value is 40%, and the content of tetracoordinated aluminum ions is Φ IV The value is 40%, and the content of tri-coordinated aluminum ions Φ III The value is 20%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 150℃ for 3h, and calcined at 480℃ for 3h to obtain hydrogenation catalyst II. The prepared catalyst II contains 12.0% MoO3, 2.5% NiO, and 85.5% alumina carrier; the properties of the catalyst are as follows: specific surface area is 175m 2 / g, and the pore diameter is 12.8nm.
[0068] The modified alumina used in the hydrogenation catalyst III was prepared by the aluminum sulfate method. After adding diethylene glycol during the kneading process, it was extruded into a plastic body, dried at 120°C for 2h, and calcined at 500°C for 3h to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared alumina carrier II was Φ V The value is 45%, and the content of tetracoordinated aluminum ions Φ IV The value is 40%, and the content of tri-coordinated aluminum ions Φ III The value is 15%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 160℃ for 4h, and calcined at 500℃ for 4h to obtain hydrogenation catalyst III. The prepared catalyst III contains 21.5% MoO3, 3.6% NiO, and 74.9% alumina carrier; the properties of the catalyst are as follows: specific surface area is 190m 2 / g, and the pore diameter is 8.7nm.
[0069] Comparative Example 3
[0070] This example provides a catalyst grading solution for long-term operation with inferior raw materials, namely, loading catalysts in the reactor, and loading hydrogenation catalyst I, hydrogenation catalyst II and hydrogenation catalyst III from top to bottom along the flow direction of the liquid reactants in the bed, wherein the loading volume ratio of hydrogenation catalysts I, II and III is 15%:45%:40%.
[0071] The modified alumina used in the hydrogenation catalyst I is prepared by carbonization method, and after being kneaded and extruded into a plastic body, it is dried at 150°C for 2 hours and calcined at 500°C for 3 hours to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 40%, and the content of tetracoordinated aluminum ions is Φ IV The value is 40%, and the content of tri-coordinated aluminum ions Φ III The value is 20%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 150°C for 3h, and calcined at 480°C for 3h to obtain hydrogenation catalyst I. The prepared catalyst I contains 6.5% MoO3, 0.7% NiO, and 92.8% alumina carrier; the properties of the catalyst are as follows: specific surface area is 220m 2 / g, and the pore diameter is 8.8nm.
[0072] The modified alumina used in the hydrogenation catalyst II is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 150°C for 2 hours and calcined at 500°C for 3 hours to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 40%, and the content of tetracoordinated aluminum ions is Φ IV The value is 40%, and the content of tri-coordinated aluminum ions Φ III The value is 20%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 150℃ for 4h, and calcined at 470℃ for 3h to obtain hydrogenation catalyst II. The prepared catalyst II contains 12.0% MoO3, 2.5% NiO, and 85.5% alumina carrier; the properties of the catalyst are as follows: specific surface area is 175m 2 / g, and the pore diameter is 8.6nm.
[0073] The modified alumina used in the hydrogenation catalyst III is prepared by carbonization method, and after being mixed and kneaded into a plastic body, it is dried at 150°C for 2 hours and calcined at 500°C for 3 hours to obtain the desired alumina carrier III. The content of pentacoordinated aluminum ions in the prepared modified alumina carrier III is Φ V The value is 40%, and the content of tetracoordinated aluminum ions is Φ IV The value is 40%, and the content of tri-coordinated aluminum ions Φ IIIThe value is 20%; the above carrier is saturated with Mo-Ni active metal solution, then dried at 150℃ for 3h, and calcined at 400℃ for 3h to obtain hydrogenation catalyst III. The prepared catalyst III contains 21.5% MoO3, 3.6% NiO, and 74.9% alumina carrier; the properties of the catalyst are as follows: specific surface area is 150m 2 / g, and the pore diameter is 8.7nm.
[0074] Example 4
[0075] This example is a comparative test of the activity and stability of the catalyst combination system of Examples 1, 2, 3 and Comparative Examples 1, 2, 3 on a 100mL fixed bed small hydrogenation device, and the feeding method adopts upper feeding. The properties of the evaluated raw oil are shown in Table 1; the evaluation conditions are shown in Table 2.
[0076] Table 1 Raw oil properties
[0077]
[0078]
[0079] Table 2 Evaluation process conditions
[0080] Reaction temperature, °C 380 Reaction hydrogen partial pressure, MPa 15.0 <![CDATA[Liquid hourly space velocity, h -1 > 0.7 Hydrogen to oil volume ratio 800:1
[0081] Table 3 Evaluation results of various catalyst combinations
[0082]
[0083] The above describes the specific implementation of the present invention in detail, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the various technical features being combined in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A catalyst grading method, characterized in that: It includes a graded system consisting of n-level catalysts, wherein n≥3, each level of catalyst comprises an alumina carrier, wherein the alumina carrier contains three types of aluminum ions: tri-coordinated aluminum ions Al 3+ Ⅲ , four-coordinated aluminum ion Al 3+ Ⅳ and pentacoordinated aluminum ion Al 3+ Ⅴ The n-level catalyst grading satisfies the following conditions: along the flow direction of the liquid phase reactant, based on the total amount of three ligands of aluminum in the alumina carrier, the content of penta-coordinated aluminum ions is The content of tri-coordinated aluminum ions decreases gradually, with a decrease of 5 to 15 percentage points. The increase is gradual, with the increment ranging from 1 to 10 percentage points.
2. The grading method according to claim 1, characterized in that: The catalyst grading method comprises a grading system consisting of n-grade catalysts, wherein n is 3 or 4.
3. The grading method according to claim 1, characterized in that: In each level of catalyst, the total content of three ligand aluminum is taken as the basis, and the content of penta-coordinate aluminum ion is The content of tetracoordinate aluminum ions is 40% to 60%. The content of tri-coordinated aluminum ions is 30% to 50%. It is 10% to 30%.
4. The grading method according to claim 1, characterized in that: In the alumina carrier of the same grade catalyst, 5. The grading method according to claim 1, characterized in that: In the alumina carrier of the same grade of catalyst, the difference between the content of penta-coordinated aluminum ions and the content of tri-coordinated aluminum ions is 15% to 50%.
6. The grading method according to claim 1, characterized in that: The graded system includes three catalysts. Based on the total volume of the catalyst in the reactor, along the flow direction of the liquid phase reactants, the three-level filling ratios are 10% to 90%: 5% to 40%: 5% to 80%, and the sum of the filling ratios of each level is 100%.
7. The grading method according to claim 1, characterized in that: The graded system includes four catalysts. Based on the total volume of the catalyst in the reactor, the four-stage filling ratios along the flow direction of the liquid reactants are: 10% to 70%: 10% to 40%: 10% to 40%: 10% to 70%, and the sum of the filling ratios of each stage is 100%.
8. The grading method according to claim 1, characterized in that: The graded system includes four catalysts. Based on the total volume of the catalyst in the reactor, the four-stage filling ratios along the flow direction of the liquid reactants are: 10% to 40%: 10% to 40%: 10% to 40%: 10% to 40%: 10% to 40%, and the sum of the filling ratios of each stage is 100%.
9. The grading method according to claim 1, characterized in that: In the catalyst, the content of the alumina carrier is 45wt% to 95wt% based on the weight of the catalyst.
10. The grading method according to claim 1, characterized in that: In the catalyst, the content of the alumina carrier is 50wt% to 95wt% based on the weight of the catalyst.
11. Use of the catalyst grading method according to any one of claims 1 to 10 in the hydroprocessing of inferior raw materials.
12. The use according to claim 11, characterized in that: The reaction conditions of the hydrotreatment are: average reaction temperature of 200°C to 450°C; reaction hydrogen partial pressure of 4.0MPa to 20.0MPa; liquid hourly volume space velocity of 0.15h -1 ~3.0h -1 ; The volume ratio of hydrogen to oil is 300~1500.
13. The use according to claim 11, characterized in that: The reaction conditions of the hydrotreatment are: average reaction temperature of 250°C to 430°C; reaction hydrogen partial pressure of 8.0MPa to 18.0MPa; liquid hourly volume space velocity of 0.2h -1 ~2.0h -1 ; The volume ratio of hydrogen to oil is 500~1200.