A single-component anti-corrosion geopolymer cement material and preparation method thereof

Through the design of single-component anti-corrosion geopolymer cement, combined with the use of layered double hydroxide corrosion inhibitor and solid sodium silicate, the corrosion problem of cement concrete in marine environment is solved, and high compressive strength and extended resistance are achieved. Corrosion cycle effects while simplifying the production process.

CN116444210BActive Publication Date: 2024-10-15GUANGXI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310367805.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-15
Estimated Expiration
2043-04-07

AI Technical Summary

Technical Problem

Existing cement concrete is prone to corrosion in the marine environment, especially the erosion problems caused by high concentrations of chloride ions. Traditional corrosion inhibitors have limited effect in the initial stage, and the preparation of two-component geopolymer cement requires a large amount of alkali activation solution, which is not conducive to convenience. chemical production.

Method used

Single-component anti-corrosion geopolymer cement is used, consisting of slag, fine sand, sodium silicate and layered double hydroxide corrosion inhibitor. Through a specific weight ratio and preparation method, the layered double hydroxide is used. The interlayer ion exchange characteristics extend the corrosion resistance period, and it is prepared by directly adding water using solid sodium silicate as an alkali activator to simplify the production process.

Benefits of technology

In the 90-day seawater environment, the anti-corrosion period is significantly extended, the compressive strength of the material and the electrochemical corrosion resistance of the steel bars are improved, and the production process is simplified to facilitate large-scale use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004167498640000011
    Figure HDA0004167498640000011
  • Figure HDA0004167498640000012
    Figure HDA0004167498640000012
Patent Text Reader

Abstract

The present invention provides a single-component anti-corrosion geopolymer cement and a preparation method thereof, belonging to the technical field of concrete materials. The single-component anti-corrosion geopolymer cement is mixed with slag, fine sand, sodium silicate, water and corrosion inhibitor, wherein the weight ratio of the raw materials is: slag 48.64%-49.21%, fine sand 19.45%-19.69%, sodium silicate 9.73%-9.84%, water 20.43%-20.67%; corrosion inhibitor 0.59%-1.75%. The single-component anti-corrosion geopolymer cement of the present invention is prepared by using a solid activator, and the activator does not need to be prepared separately during the operation process. The obtained cement has the good performance of low carbon and environmental protection, good corrosion resistance and high compressive strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cement preparation, in particular to a single-component corrosion-resistant geopolymer cement and a preparation method thereof. Background Art

[0002] The marine environment is a harsh and complex corrosive environment, and the high concentration of chloride ions in it is one of the main factors affecting the durability of reinforced concrete in marine engineering. As the immersion cycle increases, chloride ions in the environment will penetrate into the concrete through capillary action, diffusion, electrochemical migration and other effects of the cement concrete structure, resulting in corrosion of the steel bars inside the cement concrete, volume expansion and surface cracking of the cement concrete. Therefore, it is urgent to develop cement materials suitable for harsh marine environments.

[0003] Geopolymer is a three-dimensional network gel with silicon-oxygen tetrahedron and aluminum-oxygen tetrahedron. It is made from natural aluminosilicate minerals or industrial solid waste (fly ash, slag, steel slag, red mud, etc.) and mixed with alkaline activator solution. Compared with traditional silicate cement, the specific three-dimensional network gel structure of geopolymer shows low chloride permeability, which is beneficial for coping with chloride salt erosion in marine engineering applications and improving the durability of the structure. However, in the marine environment for a long time, corrosive ions can easily destroy the gel structure, such as Cl in the solution. - and CO2 will attack the hydration product C-(A)-SH of slag, causing decalcification of the hydration product and thus destroying the gel structure. Therefore, in order to cope with long-term corrosive environments, corrosion inhibitors must be added to geopolymer cement materials.

[0004] Currently, most of the corrosion inhibitors on the market are added with nitrite to reduce the corrosion of chloride ions on cementitious materials. However, this type of rust inhibitor can only have an anti-corrosion effect when the content of corrosive ions in the cementitious materials is sufficient, which poses a challenge to traditional corrosion inhibitors. Layered double hydroxides (LDHs) are a new type of intelligent corrosion inhibitor with interlayer ion exchange properties. They can release anti-corrosion ions and adsorb Cl in the environment in the initial stage. - , improve the initial corrosion threshold. In addition, geopolymer cement is currently divided into two-component and single-component geopolymer cement according to the preparation method. Generally, it is prepared by two-component method, that is, it is obtained by adding water to two components of alkali-activated solution and solid silicate raw material. However, in practical applications, the preparation of two-component geopolymer cement requires the preparation of a large amount of alkali-activated solution, which is not conducive to convenient production. The single-component geopolymer cement is made of solid alkali and solid silicate as raw materials, which can be obtained by directly adding water, which is convenient for large-scale use. Therefore, the development of a single-component corrosion-resistant geopolymer cement has good application prospects. Summary of the invention

[0005] The purpose of the present invention is to provide a single-component anti-corrosion geopolymer cement with good corrosion resistance and high compressive strength and a preparation method thereof in view of the serious corrosion damage of existing cement concrete in marine environment.

[0006] The technical scheme of the present invention is to provide a single-component anti-corrosion geopolymer cement, the components and weight ratio of which are: 48.64%-49.21% of slag, 19.45%-19.69% of fine sand, 9.73%-9.84% of sodium silicate, 20.43%-20.67% of water; and 0.59%-1.75% of corrosion inhibitor.

[0007] The slag is from Beihai Chengde Nickel Industry Co., Ltd., with an average particle size of D 50 =8.5μm.

[0008] The fine sand is quartz sand with a mesh size of 180-200.

[0009] The modulus of the sodium silicate is 2.0±0.1, the sodium oxide content is 25.5-29.0wt.%, and the silicon dioxide content is 49.0-53.0wt.%.

[0010] The corrosion inhibitor is layered double hydroxide.

[0011] The concentration ratio of sodium aluminate: nickel nitrate nonahydrate: alanine in the corrosion inhibitor is controlled to be 1:2:2.

[0012] The layered double hydroxide is prepared as follows:

[0013] (1) 0.02 mol sodium aluminate, 0.04 mol alanine, and 0.15 mol sodium hydroxide were placed in a beaker containing 100 ml of deionized water and stirred until dissolved. The mixture was then added to a three-necked flask fixed on a water bath reaction pot, and a rotor was placed in the three-necked flask;

[0014] (2) 0.04 mol of nickel nitrate nonahydrate was placed in a beaker containing 100 ml of deionized water and stirred until dissolved, and then added to a constant pressure burette fixed on a three-necked flask. The upper end of the burette was plugged with a glass stopper coated with vacuum silicone grease, and the other two ports of the three-necked flask were plugged with a vent tube coated with vacuum silicone grease. The vent tube was used to pass nitrogen to ensure that air was removed during the reaction process;

[0015] (3) Add nickel nitrate nine hydrate in the constant pressure burette evenly into the three-necked flask, set the temperature to 60° C., adjust the speed of the bath reaction pot to 200 r / min, and continue stirring for 6 hours;

[0016] (4) washing the reaction product with deionized water three times using a centrifuge and centrifuging at a speed of 4500 r / min for 4 min;

[0017] (5) The precipitated product was dried under vacuum at 60°C and then ground through a 200-mesh sieve.

[0018] The method for preparing the single-component corrosion-resistant geopolymer cement comprises the following steps:

[0019] (1) adding slag, fine sand and sodium silicate in weight ratios of 48.64%-49.21%, 19.45%-19.69% and 9.73%-9.84% to the mortar in turn and dry mixing for 30 seconds to make the base materials uniformly mixed;

[0020] (2) Evenly mix 0.59%-1.75% of corrosion inhibitor and 20.43%-20.67% of water in a weight ratio and add them to the above-mentioned base material, and continue to stir rapidly for 2 minutes until all materials are evenly dispersed to obtain a single-component anti-corrosion geopolymer cement material.

[0021] The present invention has the following beneficial effects:

[0022] The raw material composition of the anti-corrosion geopolymer cement material has a corrosion inhibitor in an appropriate proportion, and the corrosion inhibitor is a layered double hydroxide, which can effectively extend the anti-corrosion period and play a good anti-corrosion role in a 90-day seawater environment. At the same time, solid sodium silicate is used as an alkali activator in the raw material composition, which can be obtained by directly adding water, which is convenient for large-scale use. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a Nyquist diagram of the electrochemical corrosion resistance test diagram of the single-component corrosion-resistant geopolymer cement material of the present invention after being immersed in a seawater environment for 90 days.

[0024] Figure 2 It is a Bode plot of the electrochemical corrosion resistance test diagram of the single-component corrosion-resistant geopolymer cement material of the present invention after being immersed in a seawater environment for 90 days. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is further described in detail below in conjunction with embodiments.

[0026] Example 1

[0027] This embodiment is an example of the preparation method of the single-component corrosion-resistant geopolymer cement described in the present invention. The raw material composition and mass percentage are: 49.21% slag, 19.69% fine sand, 9.84% sodium silicate, 0.59% corrosion inhibitor, and 20.67% water.

[0028] The slag was purchased from Beihai Chengde Nickel Industry Co., Ltd., with an average particle size of D50=8.5μm; the fine sand was quartz sand of 180-200 mesh; the sodium silicate modulus was 2.0±0.1, with a sodium oxide content of 25.5-29.0wt.%, and a silicon dioxide content of 49.0-53.0wt.%; and the corrosion inhibitor was layered double hydroxide.

[0029] The method for preparing the single-component corrosion-resistant geopolymer cement comprises the following steps:

[0030] (1) Slag, fine sand, and sodium silicate with a weight ratio of 49.21%, 19.69%, and 9.84% were added to the mortar in sequence and dry mixed for 30 seconds to ensure that the base materials were evenly mixed;

[0031] (2) 0.59% by weight of corrosion inhibitor and 20.67% by weight of water are uniformly mixed and added to the above-mentioned base material, and the mixture is stirred rapidly for 2 minutes until all the materials are uniformly dispersed to obtain a single-component anti-corrosion geopolymer cement material.

[0032] Wherein, the corrosion inhibitor is a prepared layered double hydroxide, and the preparation method is as follows:

[0033] Step S1: 0.02 mol sodium aluminate, 0.04 mol alanine and 0.15 mol sodium hydroxide are placed in a beaker filled with 100 ml of deionized water and stirred until dissolved. The mixture is then added to a three-necked flask fixed on a water bath reaction pot and a rotor is placed in the three-necked flask.

[0034] Step S2: 0.04 mol of nickel nitrate nonahydrate is placed in a beaker filled with 100 ml of deionized water and stirred until dissolved, and then added to a constant pressure burette fixed on a three-necked flask, and a glass stopper coated with vacuum silicone grease is plugged on the upper end of the burette. The other two ports of the three-necked flask are plugged with vent pipes coated with vacuum silicone grease, and the vent pipes are used to pass nitrogen to ensure that air is removed during the reaction process.

[0035] Step S3: uniformly drop the nickel nitrate nonahydrate in the constant pressure burette into the three-necked flask. Set the temperature to 60° C., adjust the speed of the bath reaction pot to 200 r / min, and continue stirring for 6 hours.

[0036] Step S4: The product after the reaction was washed three times by centrifugation with deionized water at a speed of 4500 r / min for 4 min.

[0037] Step S5: The precipitated product was dried under vacuum at 60°C and then ground through a 200-mesh sieve.

[0038] Example 2

[0039] This embodiment is another example of the preparation method of the single-component corrosion-resistant geopolymer cement described in the present invention. The raw material composition and mass percentage are: 48.92% slag, 19.57% fine sand, 9.84% sodium silicate, 1.17% corrosion inhibitor, and 20.55% water.

[0040] The slag was purchased from Beihai Chengde Nickel Industry Co., Ltd., with an average particle size of D50=8.5μm; the fine sand was quartz sand of 180-200 mesh; the sodium silicate modulus was 2.0±0.1, with a sodium oxide content of 25.5-29.0wt.%, and a silicon dioxide content of 49.0-53.0wt.%; and the corrosion inhibitor was layered double hydroxide.

[0041] The method for preparing the single-component corrosion-resistant geopolymer cement comprises the following steps:

[0042] (1) Slag, fine sand, and sodium silicate with a weight ratio of 48.92%, 19.57%, and 9.84% were added to the mortar in sequence and dry mixed for 30 seconds to ensure that the base materials were evenly mixed;

[0043] (2) 1.17% by weight of corrosion inhibitor and 20.55% by weight of water are uniformly mixed and added to the above-mentioned base material, and the mixture is stirred rapidly for 2 minutes until all the materials are uniformly dispersed to obtain a single-component anti-corrosion geopolymer cement material.

[0044] Wherein, the corrosion inhibitor is a prepared layered double hydroxide, and the preparation method is the same as that in Example 1.

[0045] Example 3

[0046] This embodiment is another example of the preparation method of the single-component corrosion-resistant geopolymer cement described in the present invention. The raw material composition and mass percentage are: 48.64% slag, 19.45% fine sand, 9.73% sodium silicate, 1.75% corrosion inhibitor, and 20.43% water.

[0047] The slag was purchased from Beihai Chengde Nickel Industry Co., Ltd., with an average particle size of D50=8.5μm; the fine sand was quartz sand of 180-200 mesh; the sodium silicate modulus was 2.0±0.1, with a sodium oxide content of 25.5-29.0wt.%, and a silicon dioxide content of 49.0-53.0wt.%; and the corrosion inhibitor was layered double hydroxide.

[0048] The method for preparing the single-component corrosion-resistant geopolymer cement comprises the following steps:

[0049] (1) Slag, fine sand, and sodium silicate with a weight ratio of 48.64%, 19.45%, and 9.73% were added to the mortar in sequence and dry mixed for 30 seconds to ensure that the base materials were evenly mixed;

[0050] (2) 1.75% by weight of corrosion inhibitor and 20.43% by weight of water are uniformly mixed and added to the above-mentioned base material, and the mixture is stirred rapidly for 2 minutes until all the materials are uniformly dispersed to obtain a single-component anti-corrosion geopolymer cement material.

[0051] Wherein, the corrosion inhibitor is a prepared layered double hydroxide, and the preparation method is the same as that in Example 1.

[0052] Comparative Example 1

[0053] This embodiment is a comparative example of the preparation method of the single-component corrosion-resistant geopolymer cement of the present invention, and the raw material composition and mass percentage are: 49.50% slag, 19.80% fine sand, 9.90% sodium silicate, and 20.80% water.

[0054] The slag was purchased from Beihai Chengde Nickel Industry Co., Ltd., with an average particle size of D50=8.5μm; the fine sand was quartz sand of 180-200 mesh; the sodium silicate modulus was 2.0±0.1, with a sodium oxide content of 25.5-29.0wt.%, and a silicon dioxide content of 49.0-53.0wt.%; and the corrosion inhibitor was layered double hydroxide.

[0055] The preparation method of a single-component anti-corrosion geopolymer cement material comprises the following steps:

[0056] (1) 49.50%, 19.80%, and 9.90% of slag, fine sand, and sodium silicate were added to the mortar in sequence and dry mixed for 30 seconds to ensure that the base materials were evenly mixed;

[0057] (2) Add 20.80% water by weight into the above-mentioned base material and stir it rapidly for 2 minutes until all materials are evenly dispersed to obtain a single-component anti-corrosion geopolymer cement material.

[0058] After curing, the samples prepared in Examples 1 to 3 of the present invention and Comparative Example 1 were subjected to compressive strength tests at 1d, 3d, 3d, and 28d, and the results are shown in Table 1. The electrochemical corrosion resistance test results after immersion in a simulated marine environment for 90d are shown in Table 1. Figure 1 and Figure 2 ,in Figure 1 is the Nyquist plot, Figure 2 For the Bode diagram.

[0059] Table 1 Compressive strength of single-component anti-corrosion geopolymer cement materials

[0060] 1d compressive strength (MPa) 3d compressive strength (MPa) 7d compressive strength (MPa) 28d compressive strength (MPa) Example 1 44.83 62.98 69.51 86.11 Example 2 45.45 63.79 70.94 89.45 Example 3 40.81 61.33 68.03 78.84 Comparative Example 1 42.93 62.20 69.43 81.64

[0061] From the test results in Table 1, it can be seen that the 28d compressive strength of Example 1 and Example 2 is 5.48% and 9.57% higher than that of Comparative Example 1, respectively, but the 28d compressive strength of Example 3 is 3.43% lower than that of Comparative Example 1. The results show that when the weight ratio of the corrosion inhibitor is 1.8%, the compressive strength performance of the material is the best.

[0062] The samples of Examples 1 to 3 and Comparative Example 1 were placed in a 3.5% sodium chloride solution to test the electrochemical corrosion resistance of the steel bars in cement. The Nyquist plot is shown in FIG. Figure 1 As shown in the figure, Figure 2 As shown. Figure 1 and Figure 2 It can be seen from the test results that the arc radius and impedance value of the samples added with corrosion inhibitors are significantly improved, among which Example 1 and Example 2 are most significantly improved compared with Comparative Example 1, indicating that the addition of corrosion inhibitors can improve the corrosion resistance of steel bars in geopolymer cement.

Claims

1. Preparation method of single-component corrosion-resistant geopolymer cement, It is characterized in that Its components and weight ratio are: slag 48.64%-49.21%, fine sand 19.45%-19.69%, sodium silicate 9.73%-9.84%, water 20.43%-20.67%, corrosion inhibitor 0.59%-1.75%; The sodium silicate has a modulus of 2.0±0.1, a sodium oxide content of 25.5-29.0 wt.%, and a silicon dioxide content of 49.0-53.0 wt.%; The method for preparing the single-component corrosion-resistant geopolymer cement comprises the following steps: (1) Add slag, fine sand, and sodium silicate in weight ratios of 48.64%-49.21%, 19.45%-19.69%, and 9.73%-9.84% to the mortar in sequence and dry mix for 30 seconds to ensure that the base materials are evenly mixed; (2) Evenly mix 0.59%-1.75% of corrosion inhibitor and 20.43%-20.67% of water in a weight ratio and add them to the above-mentioned base material. Continue to stir rapidly for 2 minutes until all materials are evenly dispersed to obtain a single-component anti-corrosion geopolymer cement material. The corrosion inhibitor is a layered double hydroxide, and the layered double hydroxide is prepared as follows: (1) Place 0.02 mol sodium aluminate, 0.04 mol alanine, and 0.15 mol sodium hydroxide in a beaker containing 100 ml of deionized water and stir until dissolved. Then add the mixture to a three-necked flask fixed on a water bath reactor and place a rotor in the flask. (2) Place 0.04 mol of nickel nitrate nonahydrate in a beaker filled with 100 ml of deionized water and stir until dissolved. Then add the solution to a constant pressure burette fixed on a three-necked flask. The upper end of the burette is plugged with a glass stopper coated with vacuum silicone grease. The other two ports of the three-necked flask are plugged with vents coated with vacuum silicone grease. The vents are used to pass nitrogen to ensure that air is removed during the reaction. (3) Add nickel nitrate nonahydrate in the constant pressure burette evenly into the three-necked flask, set the temperature to 60°C, adjust the speed of the bath reactor to 200 r / min, and continue stirring for 6 hours; (4) Wash the reaction product with deionized water three times using a centrifuge and centrifuge at a speed of 4500 r / min for 4 min; (5) The precipitated product was dried in vacuum at 60°C and then ground through a 200-mesh sieve.

2. The method for preparing the single-component corrosion-resistant geopolymer cement according to claim 1, It is characterized in that The average particle size of the slag is D 50 =8.5 μm.

3. The method for preparing the single-component anti-corrosion geopolymer cement according to claim 1, It is characterized in that The fine sand is quartz sand with a mesh size of 180-200.