A method for preparing lightweight and high-strength foamed concrete by carbonizing high-calcium solid waste
The combination of particle size gradation and carbonization treatment of steel slag slurry and cement, combined with specific additives, solves the problems of low early strength and poor stability of foam concrete, significantly improves its compressive and flexural strength, and realizes the improvement of steel slag Efficient resource utilization and environmental protection effects.
Patent Information
- Application Number
- CN202310194063.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-03
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-03-03
AI Technical Summary
Foam concrete has low early strength and poor stability, which affects its compressive strength and flexural strength. The hydration activity of steel slag is relatively low, resulting in poor application results in foam concrete.
By providing micron-sized and nano-sized steel slag slurry with particle size gradation, carbonization treatment and combination with cement and other components, wet grinding and carbonization technology is used, combined with specific additives such as triethanolamine and crystal stabilizers, to form a highly active Aragonite whiskers promote hydration reaction and foam structure optimization.
It significantly improves the early strength and stability of foam concrete, enhances the compressive strength and flexural strength, realizes efficient resource utilization of steel slag, and reduces energy consumption and environmental pollution.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of building materials, and in particular to a method for preparing lightweight and high-strength foamed concrete by carbonizing high-calcium solid waste. Background Art
[0002] Foamed concrete refers to a lightweight concrete that uses cement-based cementitious materials, admixtures, etc. as the main cementitious materials, adds admixtures and water to make slurry, foams with a foaming agent, and is cast and cured. Compared with ordinary concrete, foamed concrete has a large number of pores inside, which makes it have the characteristics of low density, low thermal conductivity, good fire resistance, and good thermal insulation. However, foamed concrete has always had the problem of long initial setting time, especially the most widely used ordinary Portland cement, which mostly sets later than 45 minutes, resulting in generally low early strength of foamed concrete. At the same time, if the foam stability is poor, the foam has burst before the initial setting of cement and other cementitious materials, then pores cannot be formed in the concrete. Therefore, how to improve the strength and foam stability of foamed concrete is the technical key to the preparation of foamed concrete.
[0003] Steel slag is one of the major solid wastes with a relatively low utilization rate in steel enterprises. The large amount of steel slag piled up not only occupies land, but also the chemical components in the steel slag will pollute the surrounding environment. Therefore, how to use steel slag with high added value has become an urgent problem to be solved in the current metallurgical industry.
[0004] Steel slag is mainly oxides formed by oxidation of elements contained in molten iron and scrap steel. Its main components are oxides such as calcium, iron, silicon, magnesium, aluminum, manganese, and phosphorus, of which CaO accounts for about 30% to 60%, SiO2 accounts for about 8% to 23%, Al2O3 accounts for about 3% to 8%, and MgO accounts for about 4% to 11%. It also contains a small amount of elemental iron. In addition to a large amount of free calcium oxide, steel slag also contains mineral phases such as tricalcium silicate (3CaO·SiO2), dicalcium silicate (2CaO·SiO2), tricalcium aluminate (3CaO·Al2O3), and tetracalcium aluminoferrite (4CaO·Al2O3·Fe2O3). It has hydraulic gel properties, and the CSH gel generated by the reaction with water has a certain strength. Therefore, steel slag can replace cement and be used in the field of foam concrete.
[0005] However, since the main components of steel slag contain relatively more inert phases, the hydration activity of steel slag is relatively low, resulting in low early strength of steel slag-based foamed concrete, which will have a negative impact on the compressive strength and flexural strength of foamed concrete. Summary of the invention
[0006] In view of this, the present application provides a method for preparing lightweight and high-strength foamed concrete by carbonizing high-calcium solid waste, which can solve the problems of low compressive strength and flexural strength of foamed concrete.
[0007] The present application provides a method for preparing lightweight and high-strength foamed concrete by carbonizing high-calcium solid waste, comprising the following steps:
[0008] A. Provide micron-grade steel slag slurry with a particle size distribution of 0.39-0.81μm and nano-grade steel slag slurry with a particle size distribution of 0.24μm-0.36μm;
[0009] B. respectively making the micron-sized steel slag slurry and the nano-sized steel slag slurry form steel slag slurry suspensions under the addition of a stabilizer, and injecting CO2 gas into the steel slag slurry suspensions for carbonization, and separating the solid phase components from the carbonization reaction product liquid to obtain carbonized micron-sized steel slag and carbonized nano-sized steel slag;
[0010] C. Prepare foamed concrete raw material components according to weight parts, namely 50-88 parts of cement, 10-40 parts of carbonized micron-grade steel slag, 2-10 parts of carbonized nano-grade steel slag, 1-2 parts of polycarboxylic acid water reducer and foaming agent, and solidify the foamed concrete raw material components to obtain lightweight and high-strength foamed concrete.
[0011] Suitable but not limiting, in step A, the method for obtaining the micron-sized steel slag slurry and the nano-sized steel slag slurry comprises the following steps:
[0012] A1. The steel slag is subjected to iron removal treatment, grinding and screening in sequence to obtain steel slag powder;
[0013] A2. Wet-grinding the steel slag powder in an auxiliary agent with water as a medium, wherein the wet-grinding is performed for a first time to obtain micron-grade steel slag slurry, and the wet-grinding is performed for a second time to obtain nano-grade steel slag slurry.
[0014] Suitably but not limitingly, in step A1:
[0015] The steel slag is steel industry waste slag; the density of the obtained steel slag powder is 3.0-3.3kg / m 3 , brown-grey in colour, with a specific surface area of 400-450m 2 / kg;
[0016] Preferably, the particle size of the steel slag powder is 20-25 μm;
[0017] Preferably, the grinding is dry grinding for 20-40 min.
[0018] Suitably but not limitingly, in step A2:
[0019] The first time is 40 minutes, and the second time is 60 minutes;
[0020] Preferably, the auxiliary agent is triethanolamine.
[0021] Suitably but not restrictively, in step A2, the wet grinding process has a ball-to-material ratio of 1:3, grinding balls of 1.0-1.2 mm, and a mill speed of 350-400 r / min.
[0022] Suitably but not restrictively, in step B, the crystal stabilizer is a mixed crystal stabilizer obtained by mixing L-lysine hydrochloride and chitosan in a weight ratio of 1:3.
[0023] Suitably but not limitingly, in step B:
[0024] The carbonization process is to inject 20% CO2 gas into the aqueous phase system at a flow rate of 1 L / min at a temperature of 80°C, and apply stirring, and the carbonization time is 10-12 hours;
[0025] Preferably, the separation of the solid phase components is specifically to first filter out the filter residue from the carbonized suspension, and then freeze-dry the filter residue.
[0026] Suitably but not restrictively, in step C, the cement is ordinary Portland cement, with a model of P·I42.5 and a water-cement ratio of 0.4.
[0027] Suitably but not restrictively, in step C, the foaming agent is prepared by the following method: adding a foaming agent to water to obtain a foaming agent solution, and obtaining foam by mechanical foaming; the selected foaming agent is a plant protein composite surfactant, and the mass ratio of the foaming agent to water is 1:60.
[0028] Suitably but not restrictively, in step C, the polycarboxylate water-reducing agent is a long side group low molecular weight polycarboxylate water-reducing agent.
[0029] This application has the following beneficial effects:
[0030] (1) Steel slag is used to replace part of cement as a cementitious material. Compared with pure cement foam concrete, the present invention is green and environmentally friendly, has low energy consumption, high strength, reduces energy waste, solidifies and seals CO2, realizes the resource utilization of solid waste, and has significant economic and environmental benefits.
[0031] (2) The method for preparing lightweight and high-strength foamed concrete by carbonizing high-calcium solid waste prepared by the present invention uses wet grinding technology. During the wet grinding process, the surface structure of the steel slag is destroyed due to the collision and extrusion between the steel slags, which promotes the dissolution of calcium ions and silicon ions in the steel slag and the entry of hydroxide ions in the solution. The particle size of the steel slag after wet grinding can reach the nanometer level, the specific surface area is increased, the activity is increased, the hydration process of the system is accelerated, and more CSH gel is generated, which improves the stability of the foam and the strength of the foamed concrete.
[0032] (3) The auxiliary agent of this application is triethanolamine, and its main functions are as follows:
[0033] First, triethanolamine, as a highly polar small molecule, interacts with Al on the surface of C3A and C4AF through acid-base interaction. 3 + , Fe 3+ The cationic groups selectively bond, significantly reducing the polar surface energy and its proportion of total surface energy; at the same time, the C-C single bond in the molecule also creates van der Waals forces between it and C3S and C2S, resulting in a reduction in the dispersion surface energy. Triethanolamine neutralizes the unsaturated charge through adsorption, reduces the surface energy of the slag powder particles, and prevents the slag particles from agglomerating and healing each other, thereby achieving a grinding aid effect;
[0034] Second, there is an unshared electron pair on the central N atom in the triethanolamine molecular structure, which can make triethanolamine react with the metal ion Fe in the slurry. 3+ 、Al 3+ Complexation occurs, increasing the solubility of metal ions in the slurry, accelerating the diffusion of metal ions in the slurry, accelerating the dissolution rate of intermediate minerals, and thus accelerating the hydration rate;
[0035] Third, triethanolamine accelerates the formation of hexagonal calcium aluminate hydrate, a hydration product of aluminate minerals, and can promote the transformation of hexagonal calcium aluminate hydrate to cubic form, further accelerating the hydration of C3A.
[0036] Fourth, triethanolamine improves the density and strength of cement paste by inhibiting the formation of a loose structure of C3A in the early stage of hydration.
[0037] (4) During the carbonization process of steel slag, Ca dissolved in the steel slag clinker 2+It reacts with CO2 to form aragonite, calcite or amorphous calcium carbonate; L-lysine hydrochloride in the solution can make calcite amorphous, while chitosan can promote the formation of aragonite whiskers. The combined use of the two can not only promote the formation of aragonite calcium carbonate but also inhibit the crystallization and precipitation of calcite calcium carbonate, affecting the mechanical properties; therefore, after carbonization, there is an amorphous phase in the steel slag rich in aragonite whiskers. Because of its large surface area, the steel slag rich in aragonite whiskers has high activity and can also serve as a nucleation site that can accelerate cement hydration. In addition, the amorphous phase has a very high volcanic ash reaction activity, which consumes the Ca in the pore solution. 2+ , which further promotes and accelerates the hydration of cement. In addition, the aragonite phase formed after the carbonization of steel slag has a certain accelerating effect on cement hydration due to the nucleation effect. Therefore, the carbonized steel slag can accelerate the hydration of cement, shorten the initial setting time of foamed concrete, and enhance its early strength.
[0038] (5) After carbonization, steel slag forms micron-sized aragonite whiskers, whose main functions are as follows:
[0039] First, micron-sized aragonite whiskers can effectively improve the compressive strength of foamed cement. Micron-sized aragonite whiskers can bond with hydration products and unhydrated products in the foamed cement matrix to form a three-dimensional network structure that plays a supporting role, thereby improving the overall strength of the foamed cement. When the foamed cement is subjected to external force, the micron-sized aragonite whiskers in the foamed cement can bear part of the energy and restrain the expansion of cracks. The whiskers spanning across the two ends of the cracks can play a connecting role and prevent the cracking of the foamed cement. At the same time, the micron-sized aragonite whiskers make the foamed concrete more dense, reduce micro cracks, and greatly improve the flexural performance of the foamed concrete.
[0040] Second, during the mixing process of the slurry, the micron-sized aragonite whiskers will divide the large bubbles into smaller bubbles, thereby reducing the pore size of the foamed cement and making the pore size more uniform. Therefore, the micron-sized aragonite whiskers can improve the compressive strength of the foamed cement by improving the pore structure of the foamed cement;
[0041] Third, due to the low surface adhesion between micron-sized aragonite whiskers and cement paste, the foamed concrete will have a higher porosity, thus obtaining a lightweight foamed concrete with a lower dry density.
[0042] (6) The nanoscale aragonite whiskers generated by carbonization of steel slag can stabilize the foam and improve the volume stability. At the same time, they can form an interpenetrating network structure with calcium silicate hydrate and enhance the micromechanical properties of the pore wall structure. DETAILED DESCRIPTION
[0043] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the embodiments of the present application. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.
[0044] In the description of the present application, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present application, "plurality" means two or more, unless otherwise clearly and specifically defined.
[0045] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or mutual communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0046] The disclosure below provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present application. In addition, the present application can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the various specific processes and material examples provided by the present application, but those of ordinary skill in the art can appreciate the application of other processes and / or the use of other materials.
[0047] <Preparation method>
[0048] This embodiment provides a method for preparing lightweight and high-strength foamed concrete by carbonizing high-calcium solid waste, comprising the following steps:
[0049] Step 1: First, the steel slag is passed through a magnetic field with a strength of 5×10 5 After iron removal by dry magnetic separator of 1000 A / m, dry grinding is performed for 20-40 minutes, and finally sieving is performed to obtain 20-25μm steel slag powder;
[0050] Step 2, mixing the steel slag with 1.5 parts of an additive and water and wet grinding the mixture for 40-60 minutes, and wet grinding the mixture for 40 minutes and 60 minutes respectively to obtain steel slag slurry with a particle size distribution of 0.39-0.81 μm and 0.24 μm-0.36 μm;
[0051] Step 3, respectively mixing the micron-sized steel slag and the nano-sized steel slag slurry with a stabilizer to prepare a steel slag slurry suspension, then injecting CO2 gas into the suspension to generate a steel slag slurry after carbonization, and finally, filtering and drying to obtain the carbonized micron-sized steel slag and nano-sized steel slag;
[0052] Step 4: Take cement, carbonized micron-sized steel slag, carbonized nano-sized steel slag, and water, add polycarboxylate water reducer, stir evenly, and obtain steel slag-cement slurry; then mix the foaming agent with water at a ratio of 1:60; finally, mix the slurry with the foam and stir evenly;
[0053] Step 5: After vibration, molding and curing, lightweight and high-strength foamed concrete is obtained.
[0054] The following examples are carried out according to the above preparation method. The difference between these specific examples is only the difference in the raw material components in step 3 as embodied in each specific example.
[0055] Embodiment 1:
[0056] The present embodiment provides a method for preparing lightweight and high-strength foamed concrete by carbonization of high-calcium solid waste. The components are calculated by weight: 60 parts of cement, 35 parts of micron-grade steel slag, 5 parts of nano-grade steel slag, 40 parts of water, 3.5 parts of foam, 1 part of crystal stabilizer MgCl2, 1.5 parts of water reducer, and 1.5 parts of additives. The carbonization time is 12 hours.
[0057] Embodiment 2:
[0058] The present embodiment provides a method for preparing lightweight and high-strength foamed concrete by carbonization of high-calcium solid waste. The components are calculated by weight: 65 parts of cement, 30 parts of micron-grade steel slag, 5 parts of nano-grade steel slag, 40 parts of water, 3.5 parts of foam, 1 part of crystal stabilizer MgCl2, 1.5 parts of water reducer, and 1.5 parts of additives. The carbonization time is 12 hours.
[0059] Embodiment 3:
[0060] The high-calcium solid waste provided in this embodiment is carbonized to prepare lightweight and high-strength foamed concrete. The components, by weight, are 70 parts of cement, 25 parts of micron-grade steel slag, 5 parts of nano-grade steel slag, 40 parts of water, 3.5 parts of foam, 1 part of crystal stabilizer MgCl2, 1.5 parts of water reducer, and 1.5 parts of additives. The carbonization time is 12 hours.
[0061] Embodiment 4:
[0062] The high-calcium solid waste provided in this embodiment is carbonized to prepare lightweight and high-strength foamed concrete. The components, by weight, are 70 parts of cement, 20 parts of micron-grade steel slag, 10 parts of nano-grade steel slag, 40 parts of water, 3.5 parts of foam, 1 part of crystal stabilizer MgCl2, 1.5 parts of polycarboxylic acid water reducer, and 1.5 parts of additives. The carbonization time is 12 hours.
[0063] Embodiment 5:
[0064] The high-calcium solid waste provided in this embodiment is carbonized to prepare lightweight and high-strength foamed concrete. The components, by weight, are 75 parts of cement, 15 parts of micron-grade steel slag, 10 parts of nano-grade steel slag, 40 parts of water, 3.5 parts of foam, 1 part of crystal stabilizer MgCl2, 1.5 parts of polycarboxylic acid water reducer, and 1.5 parts of additives. The carbonization time is 12 hours.
[0065] Embodiment 6:
[0066] The high-calcium solid waste provided in this embodiment is carbonized to prepare lightweight and high-strength foamed concrete. The components, by weight, are 80 parts of cement, 10 parts of micron-grade steel slag, 10 parts of nano-grade steel slag, 40 parts of water, 3.5 parts of foam, 1 part of crystal stabilizer MgCl2, 1.5 parts of water reducer, and 1.5 parts of additives. The carbonization time is 12 hours.
[0067] Comparative Example 1
[0068] The only difference from Example 1 is that the particle size distribution of the steel slag slurry obtained in step 2 is 2.4 μm.
[0069] Comparative Example 2
[0070] The only difference from Example 1 is that the particle size distribution of the steel slag slurry obtained in step 2 is 0.10 μm.
[0071] Comparative Example 3
[0072] The only difference from Example 1 is that the amount of nano-grade steel slag is 15 parts.
[0073] Comparative Example 4
[0074] The only difference from Example 1 is that the amount of nano-grade steel slag is 0.5 parts.
[0075] After the foamed concrete prepared in the above embodiments and comparative examples was dried to constant weight, the compressive strength, dry density, flexural strength and crack length rate were tested according to the standard JC / T2357-2016 "Test Method for Performance of Foamed Concrete Products". The specific results are shown in Table 1 below.
[0076] Table 1 Test results of Examples 1-6 and Comparative Examples 1-4 of the present application
[0077]
[0078]
[0079] In summary, the embodiments of the present invention have the following beneficial effects: the lightweight and high-strength foamed concrete prepared in embodiments 1-6 of the present invention has the characteristics of high compressive strength and flexural strength. At the same time, due to the toughening effect of aragonite fiber, the foamed concrete products have good crack resistance and can be applied to the production of new wall materials.
[0080] The above is only a preferred specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed in the present application should be covered within the protection scope of the present application.
Claims
1. A method for preparing foamed concrete by carbonizing solid waste, characterized in that: The following steps are involved: A. Provide micron-grade steel slag slurry with a particle size distribution of 0.39-0.81μm and nano-grade steel slag slurry with a particle size distribution of 0.24μm-0.36μm; B. respectively making the micron-sized steel slag slurry and the nano-sized steel slag slurry form steel slag slurry suspensions under the addition of a stabilizer, and injecting CO2 gas into the steel slag slurry suspensions for carbonization, and separating the solid phase components from the carbonization reaction product liquid to obtain carbonized micron-sized steel slag and carbonized nano-sized steel slag; C. preparing raw material components of foamed concrete according to weight parts, namely 50-88 parts of cement, 10-40 parts of carbonized micron-grade steel slag, 2-10 parts of carbonized nano-grade steel slag, 1-2 parts of polycarboxylate water-reducing agent and foaming agent, and solidifying and molding the raw material components of foamed concrete to obtain foamed concrete; In step B, the stabilizer is a mixed crystal stabilizer obtained by mixing L-lysine hydrochloride and chitosan in a weight ratio of 1:
3.
2. The preparation method according to claim 1, characterized in that: In step A, the method for obtaining the micron-sized steel slag slurry and the nano-sized steel slag slurry comprises the following steps: A1. The steel slag is subjected to iron removal treatment, grinding and screening in sequence to obtain steel slag powder; A2. Wet-grinding the steel slag powder in an auxiliary agent with water as a medium, wherein the wet-grinding is performed for a first time to obtain micron-grade steel slag slurry, and the wet-grinding is performed for a second time to obtain nano-grade steel slag slurry.
3. The preparation method according to claim 2, characterized in that: In step A1: The steel slag is steel industry waste slag; the density of the obtained steel slag powder is 3.0-3.3kg / m 3 , brown-grey in colour, with a specific surface area of 400-450m 2 / kg; The particle size of the steel slag powder is 20-25 μm; The grinding is dry grinding for 20-40 minutes.
4. The preparation method according to claim 2, characterized in that: In step A2: The first time is 40 minutes, and the second time is 60 minutes; The auxiliary agent is triethanolamine.
5. The preparation method according to claim 2, characterized in that: In step A2, during the wet grinding process, the ball-to-material ratio is 1:3, the grinding balls are 1.0-1.2 mm, and the mill speed is 350-400 r / min.
6. The preparation method according to claim 1, characterized in that: In step B: The carbonization process is to inject 20% CO2 gas into the aqueous phase system at a flow rate of 1 L / min at a temperature of 80°C and apply stirring for a carbonization time of 10-12 hours; The separation of the solid phase components specifically includes first filtering out filter residues from the carbonized suspension, and then freeze-drying the filter residues.
7. The preparation method according to claim 1, characterized in that: In step C, the water-to-binder ratio is 0.
4.
8. The preparation method according to claim 1, characterized in that: In step C, the foaming agent is prepared by the following method: adding the foaming agent into water to obtain a foaming agent solution, and obtaining foam by mechanical foaming; the selected foaming agent is a plant protein composite surfactant, and the mass ratio of the foaming agent to water is 1:
60.
9. The preparation method according to claim 1, characterized in that: In step C, the polycarboxylate water-reducing agent is a long side group low molecular weight polycarboxylate water-reducing agent.