A high performance cement stabilized aggregate and preparation method thereof

By using specific raw materials and proportional preparation in cement-stabilized aggregates, the problem of cement-stabilized aggregates being sensitive to temperature and humidity is solved, and its crack resistance and strength are improved, the service life is extended and the rolling resistance of the road surface is improved. .

CN116444238BActive Publication Date: 2024-11-26HANGZHOU HANGHONG CONSTR TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310373969.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-11-26
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

Cement stable aggregate is sensitive to temperature and humidity, has poor resistance to shrinkage and deformation, resulting in cracks, affecting the quality and service life of the road surface.

Method used

Use bauxite cement, coarse aggregate, fine aggregate, silicone resin solution, glue powder, methyl methacrylate, lightly sintered magnesium oxide-calcium oxide composite expansion agent and magnesium hydrazite fiber and other raw materials to be uniformly mixed and specific Proportional preparation improves the crack resistance and strength of cement stabilized aggregates.

Benefits of technology

It significantly improves the crack resistance and strength of cement stable aggregates, reduces crack generation, extends service life, and improves the rolling resistance and stability of the road surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004169635070000041
    Figure BDA0004169635070000041
  • Figure BDA0004169635070000051
    Figure BDA0004169635070000051
  • Figure BDA0004169635070000052
    Figure BDA0004169635070000052
Patent Text Reader

Abstract

The present application relates to the technical field of cement stabilized materials, and specifically discloses a high-performance cement stabilized aggregate and a preparation method thereof, a cement stabilized aggregate, which comprises the following raw materials in parts by weight: 150-300 parts of alumina cement, 80-85 parts of coarse aggregate, 10-20 parts of fine aggregate, 4-8 parts of silicone resin solution, 4-8 parts of rubber powder, 1-3 parts of methyl methacrylate, 0.5-0.7 parts of light-burned magnesium oxide-calcium oxide composite expansion agent, 2-8 parts of brucite fiber and 130-150 parts of water. The 7d unconfined compressive strength and 25°C working life of the cement stabilized aggregate obtained in the present application are 6.71MPa and 14589 times at the highest, respectively, and the average temperature shrinkage coefficient and average dry shrinkage coefficient are 11.00×10 ‑6 and 46.10×10 ‑6 , which improves the crack resistance and strength of cement-stabilized aggregate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of cement stabilized materials, and more specifically, to a high-performance cement stabilized aggregate and a preparation method thereof. Background Art

[0002] Cement stabilized aggregate refers to a mixture of loose soil, sand or other aggregates with an appropriate amount of cement and water. After paving, rolling and curing, cement stabilized aggregate can be used in highway construction to obtain a cement stabilized base with high strength and good water stability.

[0003] In the related technology, cement-stabilized aggregate has a certain degree of brittleness and is sensitive to temperature and humidity, resulting in poor resistance to shrinkage and deformation of cement-stabilized aggregate, causing cracks. The cracks will reflect upward, causing corresponding reflective cracks in the asphalt binder surface layer, resulting in lower road quality and shortened service life. Summary of the invention

[0004] In order to improve the crack resistance of cement stabilized aggregate, the present application provides a high-performance cement stabilized aggregate and a preparation method thereof.

[0005] In the first aspect, the present application provides a high-performance cement-stabilized aggregate, which adopts the following technical solution:

[0006] A high-performance cement-stabilized aggregate is prepared from the following raw materials in parts by weight: 150-300 parts of alumina cement, 80-85 parts of coarse aggregate, 10-20 parts of fine aggregate, 4-8 parts of silicone resin solution, 4-8 parts of rubber powder, 1-3 parts of methyl methacrylate, 0.5-0.7 parts of light-burned magnesia-calcium oxide composite expansion agent, 2-8 parts of brucite fiber and 130-150 parts of water.

[0007] By adopting the above technical solution, the shrinkage value of alumina cement is small, which can reduce the cracks in cement-stabilized aggregate caused by excessive shrinkage of cement.

[0008] Coarse aggregate plays a role as a skeleton support in cement-stabilized aggregate. The addition of fine aggregate fills the gaps in the coarse aggregate, improves the density of the cement-stabilized aggregate, and thus improves the rolling resistance of the cement-stabilized aggregate.

[0009] Adding silicone resin solution and rubber powder is beneficial to filling the voids in cement-stabilized aggregate, reducing microcracks on the surface of coarse aggregate and fine aggregate, improving its overall structural strength, and reducing the porosity of cement-stabilized aggregate, so that cement-stabilized aggregate is not prone to shrinkage cracks due to water evaporation during use. In addition, silicone resin solution and rubber powder can play a good compounding and synergistic role when used, which can not only greatly improve the structural strength and stability of recycled aggregate, but also improve the bonding strength between the various component raw materials, thereby improving the crack resistance of cement-stabilized aggregate.

[0010] The addition of methyl methacrylate can improve the dispersibility of rubber powder in the cement stabilized aggregate system, thereby increasing the bonding strength between the various component raw materials, thereby improving the crack resistance of the cement stabilized aggregate.

[0011] Calcium oxide and light-burned magnesium oxide are processed into a light-burned magnesium oxide-calcium oxide composite expansion agent and added. After the calcium oxide crystals are hydrated, calcium hydroxide crystals are formed, and the volume increases, so as to improve the strength and rigidity of cement-stabilized aggregates, and can effectively inhibit the early shrinkage cracks of cement-stabilized aggregates. However, the calcium oxide expansion agent requires a large amount of water for hydration, and the hydration is fast, so the compensation effect for the later shrinkage is not large. The magnesium oxide expansion agent requires less water for hydration, and the hydration product is more stable and the hydration speed is slow, so the compensation effect for the later shrinkage of cement-stabilized aggregates is greater. Therefore, calcium oxide and light-burned magnesium oxide are used in combination to improve the expansion effect of the expansion agent; in addition, the light-burned magnesium oxide-calcium oxide composite expansion agent can also increase the thermal shrinkage coefficient of cement-stabilized aggregates, thereby improving crack resistance.

[0012] Brucite fiber is a non-asbestos mineral fiber with excellent mechanical properties and dispersibility. Adding brucite fiber can serve as the main body to bear external loads, reduce the shrinkage deformation of cement-stabilized aggregate, and improve crack resistance. At the same time, brucite fiber can also improve the bending strength and fatigue resistance of cement-stabilized aggregate.

[0013] Preferably: a high-performance cement-stabilized aggregate, 200-250 parts of alumina cement, 82-84 parts of coarse aggregate, 14-18 parts of fine aggregate, 5-7 parts of silicone resin solution, 5-7 parts of rubber powder, 1.5-2.5 parts of methyl methacrylate, 0.55-0.65 parts of light-burned magnesium oxide-calcium oxide composite expansion agent, 4-7 parts of brucite fiber and 135-145 parts of water. Preferably: the light-burned magnesium oxide-calcium oxide composite expansion agent is prepared by the following steps: calcium oxide and light-burned magnesium oxide are mixed in a mass ratio of 1: (2-4), calcined at 950-1050°C, and cooled to obtain the light-burned calcium oxide-magnesium oxide composite expansion agent.

[0014] By adopting the above technical scheme, light-burned magnesium oxide and calcium oxide are calcined at 950-1050° C., the activity value of magnesium oxide is increased, thereby improving the expansion performance of the light-burned magnesium oxide-calcium oxide composite expansion agent in cement stabilized aggregate.

[0015] Preferably, the high-performance cement-stabilized aggregate further comprises the following raw materials in parts by weight: 0.01-0.03 parts of styrene-butadiene latex powder.

[0016] By adopting the above scheme, the addition of styrene-butadiene latex powder can improve the density, bonding force and strength of cement-stabilized aggregate, thereby reducing the occurrence of cracks in cement-stabilized aggregate and improving the crack resistance of cement-stabilized aggregate.

[0017] Preferably, the high performance cement further comprises 0.05-0.07 parts by weight of sodium hexametaphosphate.

[0018] By adopting the above technical solution, the addition of sodium hexametaphosphate can further improve the dispersibility of styrene-butadiene latex powder in the cement stabilized aggregate system, thereby improving the crack resistance of the cement stabilized aggregate.

[0019] Preferably, the coarse aggregate is at least one of granite crushed stone, basalt crushed stone and limestone crushed stone.

[0020] Preferably, the fine aggregate is at least one of natural sand, asbestos powder, stone chips and fly ash.

[0021] In a second aspect, the present application provides a method for preparing any of the above-mentioned high-performance cement-stabilized aggregates, which is specifically achieved through the following technical solutions:

[0022] A method for preparing high-performance cement-stabilized aggregate comprises the following steps:

[0023] Alumina cement, coarse aggregate, fine aggregate and 20% water are mixed uniformly to obtain a mixture A;

[0024] Add the remaining raw materials into mixture A, mix and stir evenly to obtain high-performance cement-stabilized aggregate.

[0025] In summary, the present application includes at least one of the following beneficial technical effects:

[0026] (1) By controlling the types and dosages of various raw materials of cement stabilized aggregate, the present application makes the 7d unconfined compressive strength and 25℃ working life of cement stabilized aggregate to be 6.12MPa and 12235 times respectively, and the average thermal shrinkage coefficient and average drying shrinkage coefficient to be 11.97×10 -6 and 49.21×10 -6 , which improves the crack resistance and strength of cement-stabilized aggregate.

[0027] (2) In this application, by adding styrene-butadiene latex powder to cement stabilized aggregate and controlling its dosage, the 7d unconfined compressive strength and 25°C working life of the cement stabilized aggregate are 6.3MPa and 12931 times respectively, and the average thermal shrinkage coefficient and average dry shrinkage coefficient are 11.72×10 -6 and 47.88×10 -6 , further improving the crack resistance and strength of cement-stabilized aggregate.

[0028] (3) In this application, sodium hexametaphosphate is added to cement stabilized aggregate on the basis of styrene-butadiene latex powder, so that the 7d unconfined compressive strength and 25°C working life of cement stabilized aggregate are 6.57MPa and 14157 times respectively, and the average thermal shrinkage coefficient and average dry shrinkage coefficient are 11.80×10 -6 and 46.25×10 -6 , which improves the crack resistance and strength of cement-stabilized aggregate.

[0029] (4) In the present application, when a light-burned magnesia-calcium oxide composite expansion agent is prepared in cement-stabilized aggregate, when the mass ratio of calcium oxide to light-burned magnesia is 1:3, the 7d unconfined compressive strength and 25°C working life of the cement-stabilized aggregate are 6.71MPa and 14589 times respectively, and the average temperature shrinkage coefficient and average dry shrinkage coefficient are 11.00×10 -6 and 46.10×10 -6 , further improving the crack resistance and strength of cement-stabilized aggregate. DETAILED DESCRIPTION

[0030] The present application is further described in detail below in conjunction with specific embodiments.

[0031] The following raw materials in the present application are all commercially available products, specifically: alumina cement, particle size is 200 mesh; limestone crushed stone, particle size is 10 mm; fly ash, particle size is 325 mesh; silicone resin solution, model SILRES KX; rubber powder, particle size is 120 mesh; methyl methacrylate, molecular weight 100.12; brucite fiber, particle size is 1-3 mm, compressive strength is 21.32 Mpa; styrene-butadiene latex powder, particle size is 80-100 mm, item number BX-3; sodium hexametaphosphate, industrial grade, effective substance content 99%.

[0032] Preparation Example 1

[0033] The light-burned magnesium oxide-calcium oxide composite expansion agent of Preparation Example 1 is prepared by the following steps: 0.3 kg of calcium oxide and 0.1 kg of light-burned magnesium oxide are mixed, calcined at 1000° C. for 40 min, and cooled to obtain a light-burned calcium oxide-magnesium oxide composite expansion agent.

[0034] Preparation Example 2

[0035] The light-burned magnesium oxide-calcium oxide composite expansion agent of Preparation Example 2 was prepared by the following steps: 0.1 kg of calcium oxide and 0.2 kg of light-burned magnesium oxide were mixed, calcined at 1000° C. for 40 min, and cooled to obtain a light-burned calcium oxide-magnesium oxide composite expansion agent.

[0036] Preparation Example 3

[0037] The light-burned magnesium oxide-calcium oxide composite expansion agent of Preparation Example 3 was prepared by the following steps: 0.1 kg of calcium oxide and 0.3 kg of light-burned magnesium oxide were mixed, calcined at 1000° C. for 40 min, and cooled to obtain a light-burned calcium oxide-magnesium oxide composite expansion agent.

[0038] Preparation Example 4

[0039] The light-burned magnesium oxide-calcium oxide composite expansion agent of Preparation Example 4 was prepared by the following steps: 0.1 kg of calcium oxide and 0.4 kg of light-burned magnesium oxide were mixed, calcined at 1000° C. for 40 min, and cooled to obtain a light-burned calcium oxide-magnesium oxide composite expansion agent.

[0040] Example 1

[0041] A high-performance cement-stabilized aggregate is prepared by the following steps:

[0042] According to the dosage in Table 1, alumina cement, coarse aggregate (limestone crushed stone), fine aggregate (fly ash) and 20% water are mixed uniformly to obtain mixture A;

[0043] Add silicone resin solution, rubber powder, methyl methacrylate, the light-burned magnesium oxide-calcium oxide composite expansion agent prepared in Preparation Example 1, brucite fiber and remaining water to mixture A, mix and stir evenly to obtain high-performance cement stabilized aggregate.

[0044] Example 2-3

[0045] The high performance cement stabilized aggregate of Example 2-3 is completely the same as that of Example 1 in terms of preparation method and raw material types, the difference being that the dosage of each raw material is different, as shown in Table 1 for details.

[0046] Table 1 Amount of each raw material of high performance cement stabilized aggregate of Examples 1-3 (unit: kg)

[0047]

[0048]

[0049] Example 4

[0050] The high-performance cement-stabilized aggregate of Example 4 is prepared in exactly the same manner and in the same raw material dosage as that of Example 2, except that styrene-butadiene latex powder is added to the raw materials of the cement-stabilized aggregate, as shown in Table 2 for details.

[0051] Embodiment 5-6

[0052] The high performance cement stabilized aggregate of Examples 5-6 is completely the same in preparation method and raw material types as that of Example 4, except that the types and dosages of the raw materials are different, as shown in Table 2 for details.

[0053] Table 2 Amount of each raw material of high performance cement stabilized aggregate of Examples 4-6 (unit: kg)

[0054]

[0055] Example 7

[0056] The high-performance cement-stabilized aggregate of Example 7 is completely the same in preparation method and raw material dosage as those of Example 2, except that sodium hexametaphosphate is added to the raw materials of the cement-stabilized aggregate, as shown in Table 3 for details.

[0057] Embodiment 8-9

[0058] The high performance cement stabilized aggregate of Examples 8-9 is completely the same as that of Example 7 in terms of preparation method and raw material types, the difference being the types and dosages of the raw materials. For details, see Table 3.

[0059] Table 3 Amount of each raw material of high performance cement stabilized aggregate of Examples 7-9 (unit: kg)

[0060]

[0061]

[0062] Example 10

[0063] The high-performance cement-stabilized aggregate of Example 10 has exactly the same preparation method and raw material dosage as those of Example 8, except that 0.02 kg of styrene-butadiene latex powder is added to the cement-stabilized aggregate raw materials, and the other raw material types and dosages are the same as those of Example 8.

[0064] Examples 11-13

[0065] The high-performance cement-stabilized aggregates of Examples 11-13 are exactly the same in preparation method and raw material dosage as those of Example 10, except that the light-burned magnesium oxide-calcium oxide composite expansion agent prepared in Preparation Examples 2-3 is added to the cement-stabilized aggregate raw materials, and the other raw material types and dosages are the same as those of Example 8.

[0066] Comparative Example 1

[0067] The preparation method of the high-performance cement-stabilized aggregate of Comparative Example 1 is exactly the same as that of Example 1, except that the light-burned magnesium oxide-calcium oxide composite expansion agent in the raw materials of the high-performance cement-stabilized aggregate is replaced by an equal amount of calcium oxide expansion agent, and the types and dosages of other raw materials are the same as those of Example 1.

[0068] Comparative Example 2

[0069] The preparation method of the high-performance cement-stabilized aggregate of Comparative Example 2 is exactly the same as that of Example 1, except that the light-burned magnesium oxide-calcium oxide composite expansion agent in the raw materials of the high-performance cement-stabilized aggregate is replaced by an equal amount of light-burned magnesium oxide expansion agent, and the types and dosages of other raw materials are the same as those in Example 1.

[0070] Comparative Example 3

[0071] The preparation method of the high-performance cement-stabilized aggregate of Comparative Example 3 is exactly the same as that of Example 1, except that methyl methacrylate is not added to the raw materials of the high-performance cement-stabilized aggregate, and the types and dosages of other raw materials are the same as those of Example 1.

[0072] Comparative Example 4

[0073] The preparation method of the high-performance cement-stabilized aggregate of Comparative Example 4 is exactly the same as that of Example 1, except that no silicone resin solution is added to the raw materials of the high-performance cement-stabilized aggregate, and the types and dosages of other raw materials are the same as those of Example 1.

[0074] Comparative Example 5

[0075] The preparation method of the high-performance cement-stabilized aggregate of Comparative Example 5 is exactly the same as that of Example 1, except that no rubber powder is added to the raw materials of the high-performance cement-stabilized aggregate, and the types and dosages of other raw materials are the same as those of Example 1.

[0076] Comparative Example 6

[0077] The preparation method of the high-performance cement-stabilized aggregate of Comparative Example 6 is exactly the same as that of Example 1, except that no brucite fiber is added to the raw materials of the high-performance cement-stabilized aggregate, and the types and dosages of other raw materials are the same as those of Example 1.

[0078] Performance Testing

[0079] The high performance cement stabilized aggregates of Examples 1-13 and Comparative Examples 1-6 were tested using the following testing methods and standards. The test results are shown in Table 4.

[0080] 7d unconfined compressive strength: According to JTGE51 T0805-2009 “Test Procedure for Inorganic Binder Stabilized Materials for Highway Engineering”, cement stabilized aggregate was made into cylindrical specimens of φ150×150mm and subjected to 7d unconfined compressive strength test.

[0081] Average thermal shrinkage coefficient: According to JTGE51 T0854-2009 “Test Procedure for Inorganic Binder Stabilized Materials for Highway Engineering”, cement-stabilized aggregate was made into cylindrical specimens of 100mm×100mm×400mm, and a 7d unconfined compressive strength test was carried out.

[0082] Average shrinkage coefficient: According to JTGE51 T0855-2009 “Test Procedure for Inorganic Binder Stabilized Materials for Highway Engineering”, cement-stabilized aggregate was made into cylindrical specimens of φ150×1500mm and subjected to a 7d unconfined compressive strength test.

[0083] Fatigue life: The fatigue performance of the water-stable base mixture was tested using the American MTS810 material fatigue testing machine. The specimen molding method used vibration molding, the vibration frequency was 30Hz, and the static pressure was 150Kpa. The specimen curing time was 3 months, the curing temperature was 25℃, and the humidity was 90%. The test load waveform was a sine wave, and the loading frequency was 100Hz. The specimen length was 30cm, the stress level was 0.7, and the three-point loading method was used. The number of repeated loadings was the fatigue life.

[0084] Table 4 Performance test results of different cement stabilized aggregates

[0085]

[0086]

[0087] The test results in Table 4 show that the 7d unconfined compressive strength and 25℃ working life of the cement stabilized aggregate obtained in the present application are 6.71MPa and 14589 times, respectively, which is relatively high in strength. At the same time, the average thermal shrinkage coefficient and average dry shrinkage coefficient of the cement stabilized aggregate in the present application are 11.0×10 -6 and 46.1×10 -6 , which improves the crack resistance of cement-stabilized aggregate.

[0088] In Examples 1-3, the 7d unconfined compressive strength and 25°C working life of the cement stabilized aggregate of Example 2 are 6.12MPa and 12235 times, respectively, both higher than those of Example 1 and Example 3, and the average temperature shrinkage coefficient and average drying shrinkage coefficient are 11.97×10 -6 and 49.21×10 -6 , which are lower than those in Example 1 and Example 3, indicating that the dosage of the light-burned magnesia-calcium oxide composite expansive agent in the cement-stabilized aggregate of Example 2 is more appropriate, which improves the crack resistance and strength of the cement-stabilized aggregate. This may be related to the composite use of calcium oxide and light-burned magnesia to improve the expansion effect of the expansive agent, thereby improving the density of the cement-stabilized aggregate, and improving the crack resistance and strength of the cement-stabilized aggregate.

[0089] In Examples 4-6, the 7d unconfined compressive strength and 25°C working life of the cement stabilized aggregate of Example 5 are 6.3 MPa and 12931 times, respectively, both higher than those of Example 4 and Example 6, and the average temperature shrinkage coefficient and average drying shrinkage coefficient are 11.72×10 -6 and 47.88×10-6 , which are lower than those in Example 4 and Example 6, indicating that the dosage of styrene-butadiene latex powder in the cement-stabilized aggregate of Example 5 is more appropriate, which improves the crack resistance and strength of the cement-stabilized aggregate. This may be related to the fact that the addition of styrene-butadiene latex powder can improve the density, bonding force and strength of the cement-stabilized aggregate, thereby reducing the occurrence of cracks in the cement-stabilized aggregate and improving the crack resistance of the cement-stabilized aggregate.

[0090] In Examples 7-9, the 7d unconfined compressive strength and 25°C working life of the cement stabilized aggregate of Example 8 are 6.54 MPa and 13156 times, respectively, both higher than those of Example 7 and Example 9, and the average temperature shrinkage coefficient and average drying shrinkage coefficient are 11.11×10 -6 and 46.31×10 -6 , which are lower than those in Example 7 and Example 9, indicating that the dosage of sodium hexametaphosphate in the cement-stabilized aggregate in Example 8 is more appropriate, which improves the crack resistance and strength of the cement-stabilized aggregate. This may be related to the fact that the addition of sodium hexametaphosphate can further improve the dispersibility of the organosilicon resin solution in the cement-stabilized aggregate system, thereby improving the crack resistance of the cement-stabilized aggregate.

[0091] Combining the performance test data of Example 8 and Example 10, it is found that the 7d unconfined compressive strength and 25°C working life of the cement stabilized aggregate of Example 10 are 6.57MPa and 14157 times, respectively, both higher than those of Example 8, and the average temperature shrinkage coefficient and average dry shrinkage coefficient are 11.80×10 -6 and 46.25×10 -6 , which are lower than those in Example 8, indicating that the addition of sodium hexametaphosphate on the basis of styrene-butadiene latex powder in the cement-stabilized aggregate in Example 10 can further improve the crack resistance and strength of the cement-stabilized aggregate. This may be related to the fact that the addition of sodium hexametaphosphate can further improve the dispersibility of styrene-butadiene latex powder in the cement-stabilized aggregate system, thereby improving the crack resistance of the cement-stabilized aggregate.

[0092] In Examples 11-13, the 7d unconfined compressive strength and 25°C working life of the cement stabilized aggregate of Example 12 are 6.71 MPa and 14589 times, respectively, both higher than those of Examples 11 and 13, and the average temperature shrinkage coefficient and average dry shrinkage coefficient are 11.00×10 -6 and 46.10×10 -6 , which are lower than those in Example 11 and Example 13, indicating that when the light-burned magnesia-calcium oxide composite expansion agent is prepared from cement-stabilized aggregate in Example 12, when the mass ratio of calcium oxide to light-burned magnesia is 1:3, the crack resistance and strength of the cement-stabilized aggregate are improved.

[0093] In addition, combining the various indicator data of Comparative Examples 1-6 and Example 1, it is found that the addition of light-burned magnesium oxide-calcium oxide composite expansion agent, methyl methacrylate, silicone resin solution, rubber powder and brucite fiber to cement stabilized aggregate in the present application improves the crack resistance and strength of cement stabilized aggregate to varying degrees.

[0094] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A high performance cement stabilized aggregate, characterized in that: The invention comprises the following raw materials in parts by weight: 150-300 parts of alumina cement, 80-85 parts of coarse aggregate, 10-20 parts of fine aggregate, 4-8 parts of organic silicon resin solution, 4-8 parts of rubber powder, 1-3 parts of methyl methacrylate, 0.5-0.7 parts of light-burned magnesium oxide-calcium oxide composite expansion agent, 2-8 parts of brucite fiber and 130-150 parts of water; The high-performance cement stabilized aggregate further comprises the following raw materials in parts by weight: 0.01-0.03 parts of styrene-butadiene latex powder and 0.05-0.07 parts of sodium hexametaphosphate; The light-burned magnesium oxide-calcium oxide composite expansion agent is prepared by the following steps: calcium oxide and light-burned magnesium oxide are mixed in a mass ratio of 1:(2-4), calcined at 950-1050° C. for 30-60 min, and cooled to obtain the light-burned magnesium oxide-calcium oxide composite expansion agent; The coarse aggregate is at least one of granite crushed stone, basalt crushed stone and limestone crushed stone; the fine aggregate is at least one of natural sand, asbestos powder, stone chips and fly ash.

2. The high performance cement stabilized aggregate according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 200-250 parts of alumina cement, 82-84 parts of coarse aggregate, 14-18 parts of fine aggregate, 5-7 parts of organic silicon resin solution, 5-7 parts of rubber powder, 1.5-2.5 parts of methyl methacrylate, 0.55-0.65 parts of light-burned magnesium oxide-calcium oxide composite expansion agent, 4-7 parts of brucite fiber and 135-145 parts of water.

3. A method for preparing high-performance cement-stabilized aggregate according to any one of claims 1-2, characterized in that: The steps include: Alumina cement, coarse aggregate, fine aggregate and 20% water are mixed uniformly to obtain mixture A; Add the remaining raw materials into mixture A, mix and stir evenly to obtain high-performance cement-stabilized aggregate.