Crack-resistant hot-melt reflective marking coating and preparation method thereof
By combining modified C5 petroleum resin and rosin resin with EVA resin and bio-based polymer materials, the component ratio was optimized, which solved the problem of cracking and peeling of hot-melt road marking paint under environmental changes, improved adhesion and reflectivity, and simplified the construction process.
Patent Information
- Application Number
- CN202411369811.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing hot-melt road marking paint is prone to cracking and peeling due to inconsistent road surface deformation under high temperature, low temperature or high pressure environments, and multi-layer paving is cumbersome to construct.
A compound of modified C5 petroleum resin, modified rosin resin and EVA resin was used, and modified with bio-based polymer materials polycaprolactone and polylactic acid. Appropriate amounts of fillers, pigments, plasticizers and glass microspheres were added to optimize the component ratio and improve the coating’s adhesion, crack resistance and reflectivity.
It improves the adhesion and crack resistance of the coating, reduces peeling and cracking, enhances the reflective effect, and is easy to apply.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to a crack-resistant hot-melt reflective road marking coating and a preparation method thereof. Background Art
[0002] With the rapid development of the national economy, the volume of transportation is increasing day by day, and traffic accidents are also increasing day by day. There are many reasons for accidents, but the poor reflective effect of traffic road markings is one of the important reasons. Therefore, in order to strengthen traffic control and reduce accidents, the Ministry of Transport requires that all highways at or above the second level must be marked with eye-catching road markings to achieve fast and slow lanes. Therefore, it is particularly important to produce high-quality and recognizable road marking paint.
[0003] At present, the most widely used road marking paint in my country is hot-melt road marking paint. Hot-melt road marking paint is mainly composed of resin, pigment, filler and glass beads. The paint needs to be heated to 180-220 ℃ during construction. The paint cools and solidifies to form a marking line. Due to its excellent properties such as fast drying, long service life, and good night-time reflective effect, hot-melt road marking paint has become the longest-used and most widely used road marking paint in my country.
[0004] The existing Chinese patent with patent number ZL200510047609.5 discloses a nano-composite hot-melt road marking paint and its preparation method. The paint improves the wear resistance and crack resistance of the road marking paint by adding nano-scale fibers, nano-scale whiskers, micro-scale fibers, micro-scale whiskers, etc. as reinforcing materials. However, the reason for the cracking of the road marking paint layer is not only the high temperature resistance, low temperature resistance and rutting resistance of the paint layer itself, but also because the road surface will deform under high temperature, low temperature or high pressure environment. Since the deformation trend of the road surface is inconsistent with the road marking paint, the road marking paint cracks or even falls off. Therefore, except that the patent only discloses the improvement of the formula of the road marking paint itself to improve the wear resistance and crack resistance of the road marking, it does not disclose the need to improve the consistency of the deformation of the road marking paint and the road surface by improving the mutual cooperation between the two, so as to overcome the cracking and falling phenomenon of the road marking paint.
[0005] The existing patent document with an application publication date of 2018.01.12 and application publication number of CN107573777A discloses a hot-melt road marking paint and a preparation method thereof, wherein the primer coating, the intermediate coating and the surface coating are combined with multiple functional additives to improve the wear resistance, crack resistance, corrosion resistance and antifouling performance of the road marking paint. However, the road marking paint needs to be laid in multiple layers during laying, and the construction is relatively cumbersome. Summary of the invention
[0006] In view of the above problems, the present invention provides a crack-resistant hot-melt reflective road marking paint and a preparation method thereof to solve the problems existing in the background technology.
[0007] The above technical objectives of the present invention are achieved through the following technical solutions: A crack-resistant hot-melt reflective road marking paint is obtained by mixing 120-190 parts of a film former, 210-320 parts of a filler, 7-8 parts of a pigment, 3-5 parts of a plasticizer and 30-55 parts of glass microbeads in parts by mass, wherein the film former is a mixture of modified C5 petroleum resin, modified rosin resin and EVA resin.
[0008] The modified C5 petroleum resin in the present invention is modified by bio-based polymer materials polycaprolactone (PCL) and polylactic acid (PLA). The modified C5 petroleum resin can reduce the surface tension of the film-forming agent, thereby improving the adhesion of the coating, solving the problems of poor durability, easy falling off and cracking of traditional hot-melt coatings.
[0009] The modified C5 petroleum resin in the present invention can be prepared by the following method: a certain mass of C5 petroleum resin is dissolved in xylene, placed in a three-necked bottle for magnetic stirring, and N2 is introduced under the condition of condensed water circulation to keep the solution temperature controlled at (92±1)°C; a small amount of benzoyl peroxide is dissolved in xylene, and then a bio-based polymer material is added, and after mixing evenly, it is transferred into a single-layer glass reactor for reaction for 5 hours. After the reaction is completed, all the solutions are poured into a beaker, and acetone is added under stirring until the precipitated white insoluble matter no longer increases and then filtered; the filtered solid is dissolved in xylene, the insoluble matter is filtered out and then washed with acetone, and the washing is repeated 3 times to ensure the purity; then acetone is used as a solvent, and an extractor is used for extraction at 70°C for 48 hours, and the solid product is dried in a drying oven at 50°C for 48 hours, and placed in a desiccator for storage for use.
[0010] The mass ratio of the C5 petroleum resin to the bio-based polymer material is 1:3, the bio-based polymer material is a mixture of polycaprolactone (PCL) and polylactic acid (PLA), and the mass ratio of polycaprolactone (PCL) to polylactic acid (PLA) is 2:1; the mass ratio of the C5 petroleum resin to xylene is 1:10; the mass ratio of the benzoyl peroxide to xylene is 1:50; and the mass ratio of acetone to xylene is 1:1.
[0011] Since C5 petroleum resin has openable pentadiene and cyclopentadiene double bonds in its molecule, bio-based polymer materials (polylactic acid and polycaprolactone) can be grafted onto its main chain under the action of the initiator benzoyl peroxide, thereby introducing the polar groups of bio-based polymer materials into C5 petroleum resin. The free radicals generated by the thermal decomposition of the initiator attack the double bonds of the main chain, thereby opening the π bonds therein, forming free radical active sites, and undergoing grafting reaction with bio-based polymer materials. The chemical reaction equation is shown below, where R is the initiator and R1 is the polylactic acid (PLA) or polycaprolactone (PCL) side chain grafted onto the main chain of C5 petroleum resin.
[0012] PCL and PLA are grafted onto C5 petroleum resin to modify it. After modification, the relative molecular weight of C5 petroleum resin is greatly improved, the relative molecular weight distribution is significantly narrowed, and the intrinsic viscosity is increased, thereby improving the adhesion of the coating.
[0013] After modification, the surface tension of the coating is reduced, and the compressive strength and wear resistance of the coating are also improved.
[0014] Furthermore, the mass ratio of the modified C5 petroleum resin, the modified rosin resin and the EVA resin is (55-80): (60-95): (5-15).
[0015] The invention adjusts the compounding ratio of modified C5 petroleum resin, modified rosin resin and EVA resin, and the crack resistance, softening point, flexibility and fluidity of the hot-melt reflective road marking paint are greatly improved, and the drying time is short and the wear resistance is excellent. By modifying the C5 petroleum resin and the rosin resin, the compatibility with other components is enhanced.
[0016] The modified rosin resin of the present invention can be prepared by the following method: 60% of rosin is added to a four-necked flask equipped with a condenser, a thermometer and a stirrer, N2 is passed, the temperature is raised to 150°C, stirring is started to melt the rosin, and the remaining 40% of rosin is added after melting, maleic anhydride is slowly added while stirring, and the temperature is raised to control the temperature at 200°C, and the reaction is carried out at this temperature for 1 hour. Then, glycerol is added at 200°C and the temperature is raised to 270°C, and the reaction is carried out for 7 hours, and the small molecular water generated by esterification is discharged while reacting. Finally, vacuum is drawn to extract the remaining small molecular compounds to obtain the modified rosin resin.
[0017] The mass of maleic anhydride is 10% of the mass of rosin, the mass of glycerol is 20% of the mass of rosin, the reaction temperature of maleic anhydride and rosin is 200°C, the reaction time is 2h, and the reaction temperature of glycerol and maleic rosin is 270°C, and the reaction time is 5h.
[0018] Natural rosin has the characteristics of water resistance, heat resistance, strong adhesion, corrosion resistance, insulation, etc., but the shortcomings of rosin such as low softening point, easy crystallization, and high brittleness cannot meet the requirements of road marking paint for thermoplastic resins. Therefore, it is necessary to modify the rosin to make it have properties such as high softening point, light color and good chemical stability. The synthesis of modified rosin resin is carried out in two steps. First, rosin reacts with maleic anhydride to generate maleic rosin. The reaction belongs to the Diels-Alder reaction (i.e., diene synthesis reaction), which is a modification of the double bonds in rosin. Compared with rosin, maleic rosin increases the functionality of the molecule, and thus has the characteristics of higher softening point, acid value, etc. Since there are two electron-withdrawing carbonyl groups on the double bond carbon of maleic anhydride, maleic anhydride and rosin can react smoothly under heating conditions without any catalyst. Secondly, the reaction of maleated rosin and glycerol to generate modified rosin resin is a polyesterification reaction, which can reduce the acid value of maleated rosin, increase its softening point, and improve its stability through esterification. The modified rosin resin can increase the softening point of the hot-melt reflective road marking paint of the present invention.
[0019] Furthermore, the filler is one or more of heavy calcium carbonate, calcium carbonate, barium sulfate, talcum powder, silica powder, and quartz sand.
[0020] Furthermore, the filler is heavy calcium carbonate, quartz sand and talcum powder, which are premixed by an air flow mixer, and then classified into three grades of fillers with larger particle size distinction by a negative pressure screening machine, and then each grade of filler is weighed separately according to an appropriate proportion and mixed by a grooved spiral ribbon classifier; the mass ratio of heavy calcium carbonate, quartz sand and talcum powder is 1:1:(1-3); after the three are mixed, the particle size control range is 40-150 mesh, of which 40-60 mesh accounts for 25%, 60-90 mesh accounts for 40%, and 90-150 mesh accounts for 35%.
[0021] Fillers can improve the heat resistance, wear resistance and bonding strength of the coating, reduce the shrinkage of the coating and prevent sticking. Quartz sand is a filler material with good wear resistance processed from quartz stone. The function of talcum powder is to improve the fluidity of the coating. The more talcum powder is added, the better the fluidity of the coating. However, if too much talcum powder is added, the surface of the coating will become sticky, the coating will not dry easily and the drying time will be long.
[0022] Taking into account the cost of manufacturing the coating, the fluidity of the coating is improved by adjusting the selection of fillers and the proportion of fillers.
[0023] Furthermore, the pigment is titanium dioxide. The pigment can cover the color of the resin and improve the mechanical strength, adhesion, light resistance and weather resistance of the coating. The present invention uses titanium dioxide, which can be prepared into white road marking paint.
[0024] Furthermore, the plasticizer is a mixture of powdered nitrile rubber and castor oil.
[0025] Phthalate plasticizers are usually used in the prior art, but phthalate plasticizers have certain harm to the environment and human body. The present invention adopts powdered nitrile rubber and castor oil to mix and prepare plasticizers, which will not cause harm to the environment and human body, and can also improve the crack resistance and flexibility of the marking paint. Nitrile rubber has good impact resistance and anti-stripping performance. In order to better play the performance of nitrile rubber, the present invention crushes the nitrile rubber into powdered nitrile rubber.
[0026] Furthermore, the mass ratio of the powdered nitrile rubber and castor oil is 1: (1-3). The crack resistance and flexibility of the road marking paint can be better improved by controlling the powdered nitrile rubber and castor oil in an appropriate ratio. If the amount of powdered nitrile rubber added is too low, the crack resistance of the road marking paint will deteriorate. If the amount of powdered nitrile rubber added is too high, the cost will increase and the flexibility of the road marking paint will be affected. Therefore, controlling the mass ratio of powdered nitrile rubber and castor oil to 1: (1-3) can better improve the crack resistance and flexibility of the road marking paint.
[0027] Furthermore, the glass microbeads are a mixture of 20-60 mesh glass microbeads and 70-120 mesh glass microbeads, and the mass ratio of the 20-60 mesh glass microbeads to the 70-120 mesh glass microbeads is (7-9):(2-4).
[0028] The particle size of glass beads is one of the factors that affect the reflective performance of the marking, so it is crucial to select glass beads with a suitable particle size. If the particle size of the glass beads is large, the embedding degree is shallow, and they are easy to become "floating beads", which are easy to fall off under the action of external forces such as wheel rolling and friction; if the particle size is small, the sinking speed is fast, and it is easy to embed all of them inside the marking. The incident light is small and cannot form effective retro-reflection, resulting in poor reflective effect. In order to improve the retro-reflective performance of the marking as much as possible, the present invention uses 20-60 mesh glass beads and 70-120 mesh glass beads for compounding. Through a suitable ratio, the retro-reflection coefficient of the marking can be maximized. When the proportion of glass beads with a smaller mesh number but a larger particle size is large, the glass beads form more effective reflections and the reflective effect of the marking is better. When the proportion of glass beads with a smaller particle size is large, the glass beads are sunk in the paint and most of the reflected light is absorbed after multiple reflections and diffuse reflections. Therefore, setting the mass ratio of 20-60 mesh glass beads to 70-120 mesh glass beads at (7-9): (2-4) can maximize the retroreflection coefficient of the marking line.
[0029] The present invention also provides a method for preparing the above-mentioned crack-resistant hot-melt reflective road marking paint, which is prepared by the following method: uniformly mixing modified C5 petroleum resin, modified rosin resin, EVA resin, filler, pigment, plasticizer and glass microbeads according to parts by mass.
[0030] In summary, the present invention has the following beneficial effects: The crack-resistant hot-melt reflective road marking paint prepared by the interaction between the components has the characteristics of good crack resistance, short drying time, suitable softening point, good flexibility, excellent wear resistance, good retroreflective performance, strong water resistance and acid and alkali resistance.
[0031] The present invention adjusts the compounding ratio of modified C5 petroleum resin, modified rosin resin and EVA resin, and the crack resistance, softening point, flexibility and fluidity of the hot-melt reflective road marking paint are greatly improved, and the drying time is short and the wear resistance is excellent. By modifying the C5 petroleum resin and the rosin resin, the compatibility with other components is enhanced. The modified C5 petroleum resin in the present invention is modified by bio-based polymer materials polycaprolactone (PCL) and polylactic acid (PLA). The modified C5 petroleum resin can reduce the surface tension of the film-forming agent, thereby improving the adhesion of the coating, solving the problems of poor durability, easy shedding and cracking of traditional hot-melt coatings. The modified rosin resin can improve the softening point of the hot-melt reflective road marking paint of the present invention.
[0032] The mass ratio of 20-60 mesh glass microbeads to 70-120 mesh glass microbeads is set at (7-9): (2-4), which can maximize the retroreflective coefficient of the marking. The anti-cracking hot-melt reflective road marking paint of the present invention is environmentally friendly and suitable for use on roads, highways, and urban roads. It can reflect light under the illumination of automobile lights at night, making the road markings more obvious and more helpful for drivers to drive at night. DETAILED DESCRIPTION
[0033] The present invention is described in detail below in conjunction with specific embodiments.
[0034] Example 1 A crack-resistant hot-melt reflective road marking paint is prepared by mixing 80 parts by mass of modified C5 petroleum resin, 60 parts by mass of modified rosin resin, 15 parts by mass of EVA resin, 320 parts by mass of filler, 8 parts by mass of titanium dioxide, 1 part by mass of powdered nitrile rubber, 2 parts by mass of castor oil and 55 parts by mass of glass microspheres.
[0035] The filler is heavy calcium carbonate, quartz sand and talcum powder, which are premixed by an air flow mixer, and then classified by a negative pressure screening machine into three grades of fillers with larger particle size distinction, and then each grade of filler is weighed respectively according to an appropriate proportion, and mixed by a slot-type spiral ribbon classifier; the mass ratio of heavy calcium carbonate, quartz sand and talcum powder is 1:1:1; after the three are mixed, 40 mesh accounts for 25%, 90 mesh accounts for 40%, and 90 mesh accounts for 35%.
[0036] The glass microbeads are a mixture of 20-mesh glass microbeads and 120-mesh glass microbeads, and the mass ratio of the 20-mesh glass microbeads to the 120-mesh glass microbeads is 7:4.
[0037] The method for preparing the crack-resistant hot-melt reflective road marking paint in the above-mentioned embodiment 1 is prepared by the following method: modified C5 petroleum resin, modified rosin resin, EVA resin, filler, titanium dioxide, powdered nitrile rubber, castor oil and glass microbeads are uniformly mixed according to parts by mass.
[0038] Example 2 A crack-resistant hot-melt reflective road marking paint is prepared by mixing 80 parts by mass of modified C5 petroleum resin, 95 parts by mass of modified rosin resin, 15 parts by mass of EVA resin, 210 parts by mass of filler, 7 parts by mass of titanium dioxide, 1.2 parts by mass of powdered nitrile rubber, 3.6 parts by mass of castor oil and 30 parts by mass of glass microspheres.
[0039] The filler is heavy calcium carbonate, quartz sand and talcum powder, which are premixed by an air flow mixer, and then classified by a negative pressure screening machine into three grades of fillers with larger particle size distinction, and then each grade of filler is weighed according to an appropriate proportion, and mixed by a slot-type spiral ribbon classifier; the mass ratio of heavy calcium carbonate, quartz sand and talcum powder is 1:1:3; after the three are mixed, 60 mesh accounts for 25%, 60 mesh accounts for 40%, and 150 mesh accounts for 35%.
[0040] The glass microbeads are a mixture of 60-mesh glass microbeads and 70-mesh glass microbeads, and the mass ratio of the 60-mesh glass microbeads to the 70-mesh glass microbeads is 9:2.
[0041] The method for preparing the crack-resistant hot-melt reflective road marking paint in the above-mentioned embodiment 2 is prepared by the following method: modified C5 petroleum resin, modified rosin resin, EVA resin, filler, titanium dioxide, powdered nitrile rubber, castor oil and glass microbeads are uniformly mixed according to parts by mass.
[0042] Example 3 A crack-resistant hot-melt reflective road marking paint is prepared by mixing 65 parts by mass of modified C5 petroleum resin, 75 parts by mass of modified rosin resin, 10 parts by mass of EVA resin, 280 parts by mass of filler, 7.5 parts by mass of titanium dioxide, 2 parts by mass of powdered nitrile rubber, 2 parts by mass of castor oil and 45 parts by mass of glass microspheres.
[0043] The filler is heavy calcium carbonate, quartz sand and talcum powder, which are premixed by an air flow mixer, and then classified by a negative pressure screening machine into three grades of fillers with larger particle size distinction, and then each grade of filler is weighed respectively according to an appropriate proportion, and mixed by a groove-type spiral ribbon classifier; the mass ratio of heavy calcium carbonate, quartz sand and talcum powder is 1:1:2; after the three are mixed, 50 mesh accounts for 25%, 75 mesh accounts for 40%, and 120 mesh accounts for 35%.
[0044] The glass microbeads are a mixture of 40-mesh glass microbeads and 100-mesh glass microbeads, and the mass ratio of the 40-mesh glass microbeads to the 100-mesh glass microbeads is 8:3.
[0045] The method for preparing the crack-resistant hot-melt reflective road marking paint in the above-mentioned embodiment 3 is prepared by the following method: modified C5 petroleum resin, modified rosin resin, EVA resin, filler, titanium dioxide, powdered nitrile rubber, castor oil and glass microbeads are uniformly mixed according to parts by mass.
[0046] Comparative Example 1 The difference from Example 3 is that in Comparative Example 1, the added amount of modified C5 petroleum resin is 95 parts, the added amount of modified rosin resin is 55 parts, and the added amount of EVA resin is 20 parts.
[0047] Comparative Example 2 The difference from Example 3 is that the filler in Comparative Example 2 is heavy calcium carbonate and quartz sand, which are premixed using an airflow mixer and then graded into two grades of fillers with larger particle size distinction using a negative pressure screening machine. Each grade of filler is weighed separately according to an appropriate proportion and mixed evenly using a slotted screw-belt classifier; the mass ratio of heavy calcium carbonate to quartz sand is 1:1; after the two are mixed, 75 mesh accounts for 65% and 120 mesh accounts for 35%.
[0048] Comparative Example 3 The difference from Example 3 is that the filler in Comparative Example 3 is heavy calcium carbonate, quartz sand and talcum powder, which are premixed by an airflow mixer, and then classified into three grades of fillers with larger particle size distinction by a negative pressure screening machine, and then each grade of filler is weighed separately according to an appropriate proportion and mixed by a grooved spiral ribbon classifier; the mass ratio of heavy calcium carbonate, quartz sand and talcum powder is 2:1:1; after the three are mixed, 50 mesh accounts for 40%, 75 mesh accounts for 25%, and 120 mesh accounts for 35%.
[0049] Comparative Example 4 The difference from Example 3 is that the glass microbeads in Comparative Example 4 are a mixture of 40-mesh glass microbeads and 100-mesh glass microbeads, and the mass ratio of the 40-mesh glass microbeads to the 100-mesh glass microbeads is 3:8.
[0050] Comparative Example 5 The difference from Example 3 is that the C5 petroleum resin in Comparative Example 5 is not modified.
[0051] Comparative Example 6 The difference from Example 3 is that in Comparative Example 6, dioctyl phthalate is used to replace powdered nitrile rubber and castor oil.
[0052] The coatings prepared in Examples 1-3 and Comparative Examples 1-2 were heated to 200° C. and then coated on the treated substrate. The total thickness was controlled between 1.5 and 2.0 mm. The specific preparation method was carried out according to the coating preparation method of GB / T1727-92.
[0053] The coating films prepared by the coatings provided in Examples 1-3 and Comparative Examples 1-2 were tested for various properties. The test results are shown in Table 1.
[0054] Table 1 Test items standard Reference Standards Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Comparative Example 6 Softening point / ℃ >80℃ Ministry of Public Security CN48-89 Standard 110 111 110 107 111 110 110 111 110 Non-stick tire drying time / min ≤15 JT / T280-2004 8 8 8 9 12 10 8 8 8 Coating appearance After the coating is cooled and solidified, there should be no wrinkles, spots, bubbles, cracks or shedding. JT / T280-2004 qualified qualified qualified qualified qualified qualified qualified qualified qualified Water resistance There should be no abnormal phenomenon after soaking in water for 24 hours JT / T280-2004 qualified qualified qualified qualified qualified qualified qualified qualified qualified Alkali resistance There should be no abnormal phenomenon after immersion in saturated lime water for 18 hours JT / T280-2004 qualified qualified qualified qualified qualified qualified qualified qualified qualified Hardness / H - GB6799-86 6H 6H 6H 5H 6H 6H 6H 6H 6H Impact resistance / cm — GB1732-93 62 63 65 57 58 59 61 59 53 Flexibility After bending on a test rod with a diameter of 5 mm, the sample should not have cracking or peeling. JT / T280-2004 qualified qualified qualified qualified qualified qualified qualified qualified qualified Adhesion ≤4 JT / T280-2004 Level 1 Level 1 Level 1 Level 1 Level 1 Level 1 Level 1 Level 3 Level 1 Wear resistance (weight loss after 200rad / 1000 load) / mg ≤40 (JM-100) rubber grinding wheel JT / T280-2004 22 23 21 34 31.2 28 29 26 24 <![CDATA[Retroreflective coefficient / mcd.lx,m 2 > White≥200 JT / T280-2004 337 334 342 317 320 326 275 325 322 Crack resistance / Surface cracks generated one year after highway construction — - few few few many few few few a lot of many In the absence of conflict, the above-mentioned embodiments and features thereof may be combined with each other.
[0055] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A crack-resistant hot-melt reflective road marking paint, characterized in that: The film-forming agent is obtained by mixing 120-190 parts of film-forming agent, 210-320 parts of filler, 7-8 parts of pigment, 3-5 parts of plasticizer and 30-55 parts of glass microbeads in parts by mass. The film-forming agent is a mixture of modified C5 petroleum resin, modified rosin resin and EVA resin.
2. The crack-resistant hot-melt reflective road marking paint according to claim 1, characterized in that: The mass ratio of the modified C5 petroleum resin, the modified rosin resin and the EVA resin is (55-80): (60-95): (5-15).
3. The crack-resistant hot-melt reflective road marking paint according to claim 1, characterized in that: The filler is one or more of heavy calcium carbonate, calcium carbonate, barium sulfate, talcum powder, silica powder and quartz sand.
4. The crack-resistant hot-melt reflective road marking paint according to claim 3, characterized in that: The filler is heavy calcium carbonate, quartz sand and talcum powder, which are premixed by an air flow mixer, and then classified into three grades of fillers with larger particle size distinction by a negative pressure screening machine. Each grade of filler is weighed according to an appropriate proportion, and mixed by a slot-type spiral ribbon classifier; the mass ratio of heavy calcium carbonate, quartz sand and talcum powder is 1:1:(1-3); after the three are mixed, the particle size control range is 40-150 meshes, of which 40-60 meshes account for 25%, 60-90 meshes account for 40%, and 90-150 meshes account for 35%.
5. The crack-resistant hot-melt reflective road marking paint according to claim 1, characterized in that: The pigment is titanium dioxide.
6. The crack-resistant hot-melt reflective road marking paint according to claim 1, characterized in that: The plasticizer is a mixture of powdered nitrile rubber and castor oil.
7. The crack-resistant hot-melt reflective road marking paint according to claim 6, characterized in that: The mass ratio of the powdered nitrile rubber to the castor oil is 1:(1-3).
8. The crack-resistant hot-melt reflective road marking paint according to claim 1, characterized in that: The glass microbeads are a mixture of 20-60 mesh glass microbeads and 70-120 mesh glass microbeads, and the mass ratio of the 20-60 mesh glass microbeads to the 70-120 mesh glass microbeads is (7-9):(2-4).
9. A method for preparing a crack-resistant hot-melt reflective road marking paint according to any one of claims 1 to 8, characterized in that: The preparation method is as follows: modified C5 petroleum resin, modified rosin resin, EVA resin, filler, pigment, plasticizer and glass microbeads are uniformly mixed according to parts by mass.
Citation Information
Patent Citations
Environment-friendly hot-melt marking coating and preparation method thereof
CN111635688A
Composite enhanced hot-melt marking paint and preparation method thereof
CN112521825A
Continuous reflective high-standard hot melt coating
CN112662267A
Bio-based high polymer material hot-melt marking coating and preparation method thereof
CN114958135A
Preparation method of novel road marking paint
CN115806761A
Cited By
Hot-melting anti-sliding continuous light-reflecting type pavement environment-friendly marking coating and preparation process thereof
CN121227212A
An environment-friendly hot-melt anti-skid and continuous reflective road pavement marking paint and a preparation process thereof
CN121227212B
Durable high-brightness anti-skid hot-melt marking coating and preparation method thereof
CN122213859A