Perfluoropolyether block solid polymer electrolyte and preparation method and application thereof

Through isocyanate-guided perfluoropolyether and polypolyol block polymer, combined with lithium-oxygen and lithium-fluorine interactions, the problems of low room temperature ionic conductivity and poor mechanical properties of solid polymer electrolyte materials in lithium batteries are solved. The application of high fluidity, self-assembled structure and high energy density energy storage devices has been realized.

CN116444760BActive Publication Date: 2024-11-08NANJING UNIV +1
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202310238245.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-13
Publication Date
2024-11-08
Estimated Expiration
2043-03-13

AI Technical Summary

Technical Problem

The solid polymer electrolyte materials of existing lithium batteries have low ionic conductivity, easy crystallization, and poor mechanical properties at room temperature, making it difficult to meet the requirements of safety, flexibility and high temperature applications at the same time.

Method used

Isocyanate-guided perfluoropolyether and polypolyol form block polymers. Through lithium-oxygen and lithium-fluoro interactions, the crystallinity of polypolyol is improved, and a high-flow and self-assembly structure is constructed to improve the ionic conductivity. and mechanical properties.

Benefits of technology

It realizes high room temperature ionic conductivity, electrochemical stability, thermal stability and flexible materials, suitable for high energy density energy storage devices, and has self-healing and good adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116444760B_ABST
    Figure CN116444760B_ABST
Patent Text Reader

Abstract

The present invention discloses a perfluoropolyether-blocked solid polymer electrolyte, which is a complex formed by a polymer of formula I and lithium ions; the structural formula of the polymer of formula I is: #imgabs0# wherein #imgabs1# is a perfluoropolyether segment, 0≤x≤20, 0≤y≤50, 0≤z≤50, 0≤q≤20, and x, y, z and q are not 0 at the same time; wherein R1 is a spacer group of two ‑NCOs in isocyanate, and R2 is a spacer group of ‑OH in an organic polyol polymer. The solid electrolyte has high ionic conductivity, excellent thermal stability, rapid self-healing properties, good recyclability, a wide potential window, good electrochemical stability, good biocompatibility, and a precise self-assembly structure at room temperature, and has excellent mechanical strength and high elongation, and has good adhesion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of new materials, and specifically relates to a perfluoropolyether-blocked solid polymer electrolyte material and a preparation method and application thereof. Background Art

[0002] Energy storage devices play an irreplaceable role in today's information age, such as providing energy for various portable electronic devices, electric vehicles or other large equipment, to facilitate people's production and life. As a representative type of energy storage device, lithium batteries have achieved successful commercialization due to their advantages such as lightweight, high specific energy and no memory effect. Electrolytes, as one of the basic elements in the construction of lithium batteries, have been widely studied in the past few decades. In order to achieve efficient ion migration, various combinations of lithium salts and organic liquid electrolytes are widely used in various lithium-based batteries to achieve rapid ion transport. However, the resulting safety risks have also been affecting its application scenarios.

[0003] The introduction of fluorine provides a new possibility for improving the safety and performance of organic liquid electrolytes. The high thermal stability of fluorine-containing electrolytes, the easy formation of solid electrolyte interphases rich in lithium fluoride, and the wide potential window are conducive to solving the flammable and explosive problems of lithium batteries and improving the operating voltage. However, the introduction of fluorine-containing materials reduces the overall conductivity. For example, when perfluoropolyether liquid oligomers are used in lithium battery electrolytes, their ability to dissolve lithium salts is limited and their ion conductivity is low, which affects the overall performance.

[0004] At the same time, as the application of lithium batteries is getting closer to people's lives, the requirements for lithium battery safety and flexibility are also increasing to adapt to its development trend of being close to the human body. How to improve the safety of organic electrolytes in lithium batteries and achieve flexibility while maintaining the overall performance of the battery is still one of the current research hotspots. Solid polymer electrolytes have the advantages of high stability, flexibility and biocompatibility, and are one of the most promising types of solid electrolytes. However, due to the easy crystallization of common solid polymer electrolytes such as polyethylene oxide (PEO) and polyacrylonitrile, their ion transport capacity at room temperature is affected, which greatly hinders their application in harsh scenarios. Although chemical cross-linking, construction of interpenetrating networks or physical doping can inhibit crystallinity and improve ionic conductivity to a certain extent, most existing solid polymer electrolytes can only be used at temperatures of 60℃ to 80℃ or even higher without the assistance of plasticizers or additives, which seriously limits their application scenarios and makes it difficult to meet safety, flexibility, operating temperature and performance requirements at the same time. Summary of the invention

[0005] In view of the problems of crystallinity, low room temperature ionic conductivity, poor mechanical properties and safety in the above-mentioned prior art, the present invention provides a perfluoropolyether block solid polymer electrolyte and its preparation method and application. It is a material formed by a block polymer formed by isocyanate-guided perfluoropolyether and polyol combined with coordinated lithium ions. The perfluoropolyether chain blocks are evenly distributed on the polymer main chain and covalently bonded to the polyol chain segments. The modification of lithium-oxygen and lithium-fluorine interactions improves the intrinsic crystallinity of the polyol, so that the material has the characteristics of high fluidity, high dielectric constant, self-assembly, high room temperature ionic conductivity, electrochemical and thermal stability, high mechanical properties, self-repairing, strong adhesion, recyclability and biocompatibility.

[0006] To achieve the above object, the present invention adopts the following technical solution:

[0007] A perfluoropolyether-blocked solid polymer electrolyte, which is a complex formed by a polymer of formula I and lithium ions; the structural formula of the polymer of formula I is:

[0008]

[0009] in, is a perfluoropolyether segment, 0≤x≤20, 0≤y≤50, 0≤z≤50, 0≤q≤20, and x, y, z and q are not 0 at the same time; wherein R 1 is the spacer group between two -NCO groups in isocyanate, R 2 It is the spacer group of -OH in the organic polyol polymer. The differences among x, y, z and q represent different chain lengths of perfluoropolyether.

[0010] The sizes of x, y, z and q vary according to the molecular weight of the perfluoropolyether chain segment and can be integers or decimals.

[0011] Preferably, R 1 for:

[0012]

[0013]

[0014] Preferably, R 2 for:

[0015]

[0016] Wherein, n is an integer.

[0017] More preferably, R 2 for:

[0018] Wherein, n is an integer.

[0019] The present invention further provides a method for preparing the above-mentioned perfluoropolyether-blocked solid polymer electrolyte, comprising the following steps:

[0020] (1) Under anhydrous and oxygen-free conditions, a hydroxyl-terminated perfluoropolyether oligomer, an isocyanate and a catalyst are reacted in an ultra-dry organic solvent at 60 to 85° C. to obtain an isocyanate-terminated perfluoropolyether;

[0021] (2) adding an organic solution of an organic polyol polymer to the isocyanate-terminated perfluoropolyether obtained in step (1) and reacting at 60 to 85° C.;

[0022] (3) When the viscosity of the reaction mixture no longer changes, adding the organic solution of lithium salt to the reaction mixture of step (2) for reaction;

[0023] Wherein, the ratio of the total molar number of hydroxyl groups of the terminal hydroxyl perfluoropolyether oligomer and the organic polyol polymer to the molar number of isocyanate groups of the isocyanate is 1:1 to 1:1.3.

[0024] Preferably, the molar ratio of the perfluoropolyether oligomer to the organic polyol polymer is 1:1.

[0025] Preferably, the molecular weight of the hydroxyl-terminated perfluoropolyether oligomer is 500 to 5000, more preferably 1000 to 3000, such as E10H or D10H.

[0026] Preferably, the relative molecular mass of the organic polyol polymer is 100-20,000, more preferably 500-10,000.

[0027] Preferably, the organic polyol polymer is polycaprolactone diol, polyethylene glycol, polytetramethylene glycol, polylactide diol or polypropylene glycol. More preferably, the organic polyol polymer is polyethylene glycol.

[0028] Preferably, the catalyst in step (1) is an organic metal catalyst or a tertiary amine catalyst.

[0029] Preferably, the reaction time in step (1) is 40 to 180 minutes.

[0030] Preferably, the organometallic catalyst is an organotin catalyst, an organozinc catalyst or an organobismuth catalyst.

[0031] Preferably, the tertiary amine catalyst is triethylamine or diethylenetriamine.

[0032] Preferably, the organic solvent described in step (1) or the solvent of the organic solution of the organic polyol polymer described in step (2) is one or more of benzene, toluene, xylene, N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran or acetonitrile.

[0033] Preferably, the reaction time in step (2) is 5 to 24 hours.

[0034] Preferably, the lithium salt is one or more of lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium hexafluorophosphate, lithium bis(oxalatoborate) or lithium difluorooxalatoborate.

[0035] The present invention also provides applications of the above-mentioned perfluoropolyether-blocked solid polymer electrolyte, which includes: preparing flexible electronic skin, flexible sensors, adhesives or lithium-based battery electrolytes.

[0036] The beneficial effects of the present invention are:

[0037] The material of the present invention inhibits the crystallization of the organic polyol polymer by embedding perfluoropolyether in the organic polyol polymer chain segment, improves the fluidity of the chain segment, and thus enhances the carrier transport capacity. In addition, the hydrogen bonding effect, dipole-dipole interaction, and lithium-oxygen weak coordination between the polymer chain segments enable the material to obtain a self-assembly structure, construct ion channels, and improve the carrier transport efficiency. On the other hand, the introduction of the perfluoropolyether chain segment improves the dielectric constant of the material while providing a strong interaction between the polymer matrix and the anions, promotes the dissociation of ion pairs, and further improves the efficiency of the material in transporting specific cations. The synergistic effect of the three enables the material to obtain a high ionic conductivity (>10 -4 S / cm), which solves the problem of low room temperature ionic conductivity of solid polymer electrolytes.

[0038] The material of the present invention has excellent thermal stability, can overcome the safety problem of flammability and explosion of existing materials, and is helpful to expand its practical application.

[0039] The material of the present invention has good recyclability and can be used in recyclable flexible batteries.

[0040] The introduction of a large number of fluorine atoms in the perfluoropolyether in the material of the present invention makes the material have a wide potential window and can be used in high energy density energy storage devices. This is because the fluorine element has good electrochemical stability, and the obtained solid electrolyte can adapt to high-voltage positive electrode materials and low-voltage negative electrode materials, greatly improving the overall energy density of the battery. At the same time, the fluorine-rich solid electrolyte interphase spontaneously formed in the device is also conducive to improving the stability of the material.

[0041] The material of the present invention utilizes lithium-oxygen coordination bonds of different densities, hydrogen bonding, and dipole-dipole interactions to regulate the mechanical properties of the polymer, and has a precise self-assembly structure, which not only solves the problems of brittleness and poor stretchability (<200%) caused by crystallization of organic polyol polymers, and the strong fluidity of perfluoropolyether that cannot form a film, but also enables the material to obtain excellent mechanical strength while also having a high stretch rate (>2000%), which is rarely reported.

[0042] The material of the present invention has good adhesion, can fit closely with the electrode, and reduces interface impedance.

[0043] The material in the present invention has the property of rapid self-repair at room temperature, and can self-repair when damaged by the outside world. When the flexible battery is damaged by the outside world or the dendrites are damaged, it can restore the original function.

[0044] The material of the present invention has good flexibility, stretchability and high mechanical strength, and is suitable for constructing flexible energy storage devices.

[0045] The material of the invention has good biocompatibility and can be implanted in vivo to function as electronic components in vivo. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 This is the Nyquist plot of the sample prepared in Example 1 in Example 15.

[0047] Figure 2 This is a conductivity comparison chart of the samples prepared in Examples 1 to 4 in Example 15.

[0048] Figure 3 This is a conductivity comparison chart of the samples prepared in Examples 5 to 8 in Example 15.

[0049] Figure 4 This is the potential window diagram of the sample prepared in Example 1 in Example 15.

[0050] Figure 5 This is a critical current density test diagram of the sample prepared in Example 1 in Example 15.

[0051] Figure 6 This is a graph of the constant current cycle test of a lithium symmetric battery of the sample prepared in Example 1 in Example 15.

[0052] Figure 7 This is the stress-strain diagram of the samples prepared in Examples 6-7 and Examples 9-10 in Example 15.

[0053] Figure 8 This is a differential scanning calorimetry test diagram of the sample prepared in Example 10 in Example 15.

[0054] Fig. 9 This is the thermogravimetric analysis diagram of the samples prepared in Examples 10 to 11 in Example 15.

[0055] Figure 10-12 This is the broadband dielectric test spectrum of the samples prepared in Examples 10 to 12 in Example 15.

[0056] Fig.13 This is an atomic force microscope characterization image of the sample prepared in Example 1 in Example 15. DETAILED DESCRIPTION

[0057] In order to further illustrate the present invention, the room temperature high ionic conductivity polymer solid electrolyte material and the preparation method thereof provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0058] Example 1

[0059] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.

[0060] 1.5 g of polyethylene glycol with a relative molecular mass of 1500 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The molar ratio of the terminal hydroxyl perfluoropolyether and polyethylene glycol was 1:1, and the ratio of the total hydroxyl number and isocyanate was 1:1. The change in the viscosity of the system was observed.

[0061] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.

[0062] When the viscosity of the reaction mixture no longer changes, 1.3 g of lithium bis(fluorosulfonyl)imide was dissolved in 5 mL of ethylene glycol dimethyl ether, and then added to the reaction system with a syringe, and stirring was continued for 1 to 2 h.

[0063] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain the perfluoropolyether block solid polymer electrolyte, which is marked as 1500-LiFSI-8:1.

[0064] Example 2

[0065] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.

[0066] 1.5 g of polyethylene glycol with a relative molecular mass of 1500 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The molar ratio of the terminal hydroxyl perfluoropolyether and polyethylene glycol was 1:1, and the ratio of the total hydroxyl number and isocyanate was 1:1. The change in the viscosity of the system was observed.

[0067] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction lasts for 10 to 15 hours.

[0068] When the viscosity of the reaction mixture no longer changes, 1.0 g of lithium bis(fluorosulfonyl)imide was dissolved in 5 mL of ethylene glycol dimethyl ether, and then added to the reaction system with a syringe, and stirring was continued for 1 to 2 h.

[0069] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain the perfluoropolyether block solid polymer electrolyte, which is marked as 1500-LiFSI-10:1.

[0070] Example 3

[0071] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.

[0072] 1.5 g of polyethylene glycol with a relative molecular mass of 1500 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The molar ratio of the terminal hydroxyl perfluoropolyether and polyethylene glycol was 1:1, and the ratio of the total hydroxyl number and isocyanate was 1:1. The change in the viscosity of the system was observed.

[0073] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.

[0074] When the viscosity of the reaction mixture no longer changes, 0.87 g of lithium bis(fluorosulfonyl)imide was dissolved in 5 mL of ethylene glycol dimethyl ether, and then added to the reaction system with a syringe, and stirring was continued for 1 to 2 h.

[0075] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain the perfluoropolyether block solid polymer electrolyte, which is marked as 1500-LiFSI-12:1.

[0076] Example 4

[0077] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.

[0078] 1.5 g of polyethylene glycol with a relative molecular mass of 1500 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The molar ratio of the terminal hydroxyl perfluoropolyether and polyethylene glycol was 1:1, and the ratio of the total hydroxyl number and isocyanate was 1:1. The change in the viscosity of the system was observed.

[0079] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.

[0080] When the viscosity of the reaction mixture no longer changes, 0.74 g of lithium bis(fluorosulfonyl)imide was dissolved in 5 mL of ethylene glycol dimethyl ether, and then added to the reaction system with a syringe, and stirring was continued for 1 to 2 h.

[0081] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain the perfluoropolyether block solid polymer electrolyte, which is marked as 1500-LiFSI-14:1.

[0082] Example 5

[0083] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.

[0084] 1.5 g of polyethylene glycol with a relative molecular mass of 1500 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The molar ratio of the terminal hydroxyl perfluoropolyether and polyethylene glycol was 1:1, and the ratio of the total hydroxyl number and isocyanate was 1:1. The change in the viscosity of the system was observed.

[0085] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.

[0086] When the viscosity of the reaction mixture no longer changes, 1.6 g of lithium bis(trifluoromethanesulfonyl)imide was dissolved in 5 mL of ethylene glycol dimethyl ether, and then added to the reaction system with a syringe, and stirring was continued for 1 to 2 h.

[0087] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain the perfluoropolyether block solid polymer electrolyte, which is marked as 1500-LiTFSI-10:1.

[0088] Example 6

[0089] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.

[0090] 1.5 g of polyethylene glycol with a relative molecular mass of 1500 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The molar ratio of the terminal hydroxyl perfluoropolyether and polyethylene glycol was 1:1, and the ratio of the total hydroxyl number and isocyanate was 1:1. The change in the viscosity of the system was observed.

[0091] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.

[0092] When the viscosity of the reaction mixture no longer changes, 1.3 g of lithium bis(trifluoromethanesulfonyl)imide was dissolved in 5 mL of ethylene glycol dimethyl ether, and then added to the reaction system with a syringe, and stirring was continued for 1 to 2 h.

[0093] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain the perfluoropolyether block solid polymer electrolyte, which is marked as 1500-LiTFSI-12:1.

[0094] Example 7

[0095] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.

[0096] 1.5 g of polyethylene glycol with a relative molecular mass of 1500 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The molar ratio of the terminal hydroxyl perfluoropolyether and polyethylene glycol was 1:1, and the ratio of the total hydroxyl number and isocyanate was 1:1. The change in the viscosity of the system was observed.

[0097] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction lasts for 10 to 15 hours.

[0098] When the viscosity of the reaction mixture no longer changes, 1.1 g of lithium bis(trifluoromethanesulfonyl)imide was dissolved in 5 mL of ethylene glycol dimethyl ether, and then added to the reaction system with a syringe, and stirring was continued for 1 to 2 h.

[0099] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain the perfluoropolyether block solid polymer electrolyte, which is marked as 1500-LiTFSI-14:1.

[0100] Example 8

[0101] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.

[0102] 1.5 g of polyethylene glycol with a relative molecular mass of 1500 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The molar ratio of the terminal hydroxyl perfluoropolyether and polyethylene glycol was 1:1, and the ratio of the total hydroxyl number and isocyanate was 1:1. The change in the viscosity of the system was observed.

[0103] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.

[0104] When the viscosity of the reaction mixture no longer changes, 0.88 g of lithium bis(trifluoromethanesulfonyl)imide was dissolved in 5 mL of ethylene glycol dimethyl ether, and then added to the reaction system with a syringe, and stirring was continued for 1 to 2 h.

[0105] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain the perfluoropolyether block solid polymer electrolyte, which is marked as 1500-LiTFSI-18:1.

[0106] Example 9

[0107] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.

[0108] 1.5 g of polyethylene glycol with a relative molecular mass of 1500 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The molar ratio of the terminal hydroxyl perfluoropolyether and polyethylene glycol was 1:1, and the ratio of the total hydroxyl number and isocyanate was 1:1. The change in the viscosity of the system was observed.

[0109] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.

[0110] When the viscosity of the reaction mixture no longer changes, 0.63 g of lithium bis(trifluoromethanesulfonyl)imide was dissolved in 5 mL of ethylene glycol dimethyl ether, and then added to the reaction system with a syringe, and stirring was continued for 1 to 2 h.

[0111] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain the perfluoropolyether block solid polymer electrolyte, which is marked as 1500-LiTFSI-25:1.

[0112] Example 10

[0113] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.

[0114] 1.5 g of polyethylene glycol with a relative molecular mass of 1500 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The molar ratio of the terminal hydroxyl perfluoropolyether and polyethylene glycol was 1:1, and the ratio of the total hydroxyl number and isocyanate was 1:1. The change in the viscosity of the system was observed.

[0115] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.

[0116] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain the perfluoropolyether block solid polymer electrolyte, which is marked as PFPE-PEG1500.

[0117] Embodiment 11

[0118] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.

[0119] 3 g of polyethylene glycol with a relative molecular mass of 3000 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The molar ratio of the terminal hydroxyl perfluoropolyether and polyethylene glycol was 1:1, and the ratio of the total hydroxyl number and isocyanate was 1:1. The change in the viscosity of the system was observed.

[0120] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.

[0121] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain the perfluoropolyether block solid polymer electrolyte, which is marked as PFPE-PEG3000.

[0122] Example 12

[0123] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 85°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.8g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 1800, 0.34g of 1,6-hexamethylene diisocyanate, 0.01g of dibutyltin dilaurate, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 85°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.

[0124] 6 g of polyethylene glycol with a relative molecular mass of 6000 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 85°C and the stirring speed was 300 r / min. The molar ratio of the terminal hydroxyl perfluoropolyether and polyethylene glycol was 1:1, and the ratio of the total hydroxyl number and isocyanate was 1:1. The change in the viscosity of the system was observed.

[0125] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.

[0126] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain the perfluoropolyether block solid polymer electrolyte, which is marked as PFPE-PEG6000.

[0127] Embodiment 13

[0128] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 65°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 2.0g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 2000, 0.58g of dicyclohexylmethane diisocyanate, 0.01g of an organic bismuth composite catalyst (BiCAT), and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 65°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.

[0129] 10 g of polyethylene glycol with a relative molecular mass of 10,000 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 65°C and the stirring speed was 300 r / min. The molar ratio of the terminal hydroxyl perfluoropolyether and polyethylene glycol was 1:1, and the ratio of the total hydroxyl number and isocyanate was 1:1.1. The change in the viscosity of the system was observed.

[0130] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.

[0131] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain the perfluoropolyether block solid polymer electrolyte, which is marked as PFPE-PEG10000.

[0132] Embodiment 14

[0133] A 100mL two-necked flask was connected to a double-row tube, and the flask was repeatedly pumped and flushed for more than three times at 75°C and in a nitrogen atmosphere, and the process lasted for 30 minutes; then 1.0g of a terminal hydroxyl perfluoropolyether oligomer with a relative molecular weight of about 1000, 0.65g of dicyclohexylmethane diisocyanate, 0.01g of triethylamine, and 3mL of ultra-dry xylene were added to the flask through a syringe, the reaction temperature was controlled to 75°C, the stirring speed was 200r / min, and the reaction was carried out for 50 minutes to obtain an isocyanate-terminated perfluoropolyether oligomer.

[0134] 0.5 g of polyethylene glycol with a relative molecular mass of 500 was dissolved in 5 mL of N,N-dimethylacetamide and then added to the above system with a syringe. The reaction temperature was maintained at 75°C and the stirring speed was 300 r / min. The molar ratio of the terminal hydroxyl perfluoropolyether and polyethylene glycol was 1:1, and the ratio of the total hydroxyl number and isocyanate was 1:1.3. The change in the viscosity of the system was observed.

[0135] After the viscosity rises, add ultra-dry N,N-dimethylacetamide to the system in small amounts and multiple times, 3 to 5 mL each time, to ensure that the system has a viscosity that can be normally stirred at 50 to 100 r / min. The reaction continues for 10 to 15 hours.

[0136] After the reaction is completed, the product is poured into a polypropylene mold and evaporated naturally. Depending on the changes in room temperature and humidity, the process lasts for 1 to 2 days. After the solvent is completely evaporated, the material is placed in a 70°C oven and dried for 24 hours to obtain the perfluoropolyether block solid polymer electrolyte, which is marked as PFPE-PEG500.

[0137] Embodiment 15

[0138] The samples obtained in Examples 1 to 8 were tested for conductivity using a stainless steel blocking electrode. The results are as follows: Figures 1 to 3 shown. Figure 1 This is a typical Nyquist plot of the sample obtained in Example 1, based on which its conductivity is calculated. Figures 2-3 The conductivity of solid polymer electrolytes with different lithium salts and different coordination ratios of the same lithium salt was compared and regulated. Compared with the polyethylene glycol material reported in the prior art (J. Mater. Chem. A, 2015, 3, 19218-19253., Nat. Rev. Mater., 2020, 5, 229-252.), the material of the present invention completely suppresses the crystallinity of the polyol and achieves extremely high room temperature ionic conductivity. This is due to the design of block copolymerization in the present invention and the excellent interfacial adhesion and contact between the electrode electrolyte.

[0139] The sample obtained in Example 1 was used to construct a lithium / solid polymer electrolyte / stainless steel battery configuration, and its stability at different potentials was tested. The results obtained are as follows: Figure 4The material of the present invention exhibits a very wide potential window, proving that it can adapt to low-voltage negative electrodes and high-voltage positive electrodes, greatly broadening its application range and the energy density of the resulting battery, which is derived from the extremely high chemical and electrochemical stability of the material of the present invention.

[0140] The sample obtained in Example 1 was used to construct a lithium / solid polymer electrolyte / lithium battery configuration, and its polarization voltage was tested at different current densities. The results are as follows: Figure 5 The material of the present invention maintains considerable stability even at high current density, demonstrating its ability to resist dendrite growth and excellent electrochemical performance.

[0141] The sample obtained in Example 1 was used to construct a lithium / solid polymer electrolyte / lithium battery configuration, and its long-term cycle stability at a constant current density was tested. The results obtained are as follows: Figure 6 When a certain current passes through the material of the present invention, the polarization voltage is kept small and the stability is kept for a long time, which indicates that the material can keep good performance in the actual use of the battery and has great practical significance.

[0142] The samples obtained in Examples 6-7, 9-10 were tested by a universal tensile machine and the following results were obtained: Figure 7 The results shown in Figure 2 show that the mechanical properties of the polymer are greatly improved after the introduction of lithium coordination into the polymer. Through reasonable regulation, its modulus can match the magnitude required for biological wear, indicating that it can be used in the fields of flexible batteries, electronic skin and implantable devices.

[0143] The sample obtained in Example 10 was subjected to differential scanning calorimetry analysis, and the results obtained were as follows: Figure 8 The material of the present invention has a very low glass transition temperature (-52.6°C), which indicates that its chain segments have strong fluidity, which helps to promote the transport of ions in the polymer bulk phase, and explains why the material of the present invention has high room temperature ionic conductivity.

[0144] The samples obtained in Examples 10 to 11 were subjected to thermogravimetric analysis and the results obtained were as follows: Fig. 9 As shown. The material of the present invention does not contain a plasticizer to promote ion transport, indicating that its high ion conductivity at room temperature is caused by the intrinsic properties of the polymer rather than the influence of other factors. At the same time, the material of the present invention has excellent thermal stability, and its decomposition temperature is higher than 200°C, which ensures the safety of the battery constructed therefrom when in use.

[0145] The samples obtained in Examples 10 to 12 were tested for broadband dielectric properties, and the results were as follows: Figures 10-12The material of the present invention has a higher dielectric constant, which helps to promote the dissociation of ion pairs in the bulk phase, thereby obtaining a higher free carrier concentration, and ultimately achieving high room temperature ionic conductivity.

[0146] The sample obtained in Example 1 was characterized by atomic force microscopy. Fig.13 The material of the present invention has a unique rod-like self-assembly structure, which helps to construct ion transmission channels at the microscopic level, and cooperates with the above-mentioned various effects to achieve high room temperature conductivity of the material of the present invention.

Claims

1. A perfluoropolyether-blocked solid polymer electrolyte, characterized in that: The solid polymer electrolyte is a complex formed by a polymer of formula I and lithium ions; the structural formula of the polymer of formula I is: ; in, It is a perfluoropolyether segment, 0≤x≤20, 0≤y≤50, 0≤z≤50, 0≤q≤20, and y and z are not 0 at the same time; wherein R1 is a spacer group of two -NCO in isocyanate, and R2 is a spacer group of -OH in an organic polyol polymer.

2. The solid polymer electrolyte according to claim 1, characterized in that R1 is: , , , , , , , , , , , , , , , , , , , , , , , , , , or .

3. The solid polymer electrolyte according to claim 1, characterized in that R2 is: A spacer group between two -OH groups in polycaprolactone diol, a spacer group between two -OH groups in polyethylene glycol, a spacer group between two -OH groups in polytetramethylene ether diol, a spacer group between two -OH groups in polylactide diol or a spacer group between two -OH groups in polypropylene glycol.

4. The method for preparing the perfluoropolyether-blocked solid polymer electrolyte according to claim 1, characterized in that: The steps include: (1) Under anhydrous and oxygen-free conditions, a hydroxyl-terminated perfluoropolyether oligomer, an isocyanate and a catalyst are reacted in an ultra-dry organic solvent at 60-85° C. to obtain an isocyanate-terminated perfluoropolyether; (2) adding an organic solution of an organic polyol polymer to the isocyanate-terminated perfluoropolyether obtained in step (1) and reacting at 60-85° C.; (3) When the viscosity of the reaction mixture no longer changes, the organic solution of lithium salt is added to the reaction mixture of step (2) for reaction; Wherein, the ratio of the total molar number of hydroxyl groups of the terminal hydroxyl perfluoropolyether oligomer and the organic polyol polymer to the molar number of isocyanate groups of the isocyanate is 1:1 to 1:1.

3.

5. The preparation method according to claim 4, characterized in that: The molecular weight of the terminal hydroxyl perfluoropolyether oligomer is 500-5000; the relative molecular weight of the organic polyol polymer is 100-20000.

6. The preparation method according to claim 5, characterized in that: The molecular weight of the terminal hydroxyl perfluoropolyether oligomer is 1000-3000; the relative molecular weight of the organic polyol polymer is 500-10000.

7. The preparation method according to claim 4, characterized in that: The organic polyol polymer is polycaprolactone diol, polyethylene glycol, polytetramethylene glycol, polylactide diol or polypropylene glycol.

8. The preparation method according to claim 4, characterized in that: The catalyst in step (1) is an organic metal catalyst or a tertiary amine catalyst.

9. The preparation method according to claim 8, characterized in that: The organic metal catalyst is an organic tin catalyst, an organic zinc catalyst or an organic bismuth catalyst; the tertiary amine catalyst is triethylamine or diethylenetriamine.

10. The preparation method according to claim 4, characterized in that: The organic solvent described in step (1) or the solvent of the organic solution of the organic polyol polymer described in step (2) is one or more of benzene, toluene, xylene, N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran or acetonitrile.

11. The preparation method according to claim 4, characterized in that: The lithium salt is one or more of lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium hexafluorophosphate, lithium bis(oxalatoborate) or lithium difluorooxalatoborate.

12. The use of the perfluoropolyether block solid polymer electrolyte according to any one of claims 1 to 3, characterized in that: The applications include: preparing flexible electronic skin, flexible sensors, adhesives or lithium-based battery electrolytes.

Citation Information

Patent Citations

  • Solid polymer electrolyte and electrochemical devices comprising same

    CN107771351A

  • Preparation method of all-solid-state fluorine-containing polymer electrolyte membrane and lithium ion battery

    CN109326822A

  • Supramolecular polymers based on high-density hydrogen bond interaction, and application thereof

    CN111635424A

  • Solid polymer electrolyte membrane and preparation method thereof

    CN111769320A

  • Fluorine-containing polyurethane solid-state composite electrolyte and preparation method thereof

    CN111786016A