Preparation method and product of polymer foam in-situ compounded with phosphorus-containing graphene oxide
Phosphorus-containing graphene oxide is prepared by reacting with liquid phosphorus-based flame retardants and compounded into polymer foam in situ. This solves the problem of insufficient flame retardant performance of graphene oxide in polymer foam and achieves more efficient flame retardancy. , heat insulation and sound absorption performance, and simplify the process and reduce costs.
Patent Information
- Application Number
- CN202310331409.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-03-31
AI Technical Summary
When existing graphene oxide is used alone as a flame retardant filler in polymer foam, its flame retardant and smoke suppression properties are limited, and the composite process is complex and costly, making it difficult to be widely used in general technical fields.
Phosphorus-containing graphene oxide is prepared by reacting with a liquid phosphorus-based flame retardant, and is compounded in-situ into the polymer foam through ultrasonic dispersion and vacuum impregnation methods to form a phosphorus/carbon integrated flame-retardant functional filler to improve the material's durability. Flame retardant, thermal insulation and sound absorption properties.
It significantly improves the limiting oxygen index value of the polymer foam, reduces the thermal conductivity and maximum smoke gas specific optical density, and achieves better flame retardant and smoke suppression, thermal insulation and sound absorption properties, while simplifying the process and reducing costs.
Smart Images

Figure CN116444854B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polymer foam, in particular to a preparation method and a product of a phosphorus-containing graphene oxide in-situ composite polymer foam. Background Art
[0002] Polymer foam material is a porous material with the advantages of low density, excellent flexibility, and impact resistance. In recent years, polymer foam materials have been widely used in various fields such as construction, household appliances, and electronic devices. With the gradual development of polymer foam materials, they have been used in ships, aerospace, electronic equipment, and many cutting-edge technology fields. At the same time, these fields have increasingly stringent requirements on the thermal insulation, fire prevention, and smoke suppression properties of materials. However, a considerable number of polymer foam materials have been greatly limited in their application due to their poor flame retardancy, flame resistance, and the release of a large amount of toxic gases when burned.
[0003] Graphene oxide is the oxide of graphene, which is a derivative of graphite obtained through a series of oxidation, ultrasonic exfoliation and other methods. Graphene oxide obtained after oxidation treatment still maintains a single-layer sheet structure, with a large specific surface area and a large π-bond conjugated structure. Graphene oxide has the characteristics of easy processing and forming three-dimensional macroscopic assembly due to its rich oxygen-containing functional groups on its sheet surface and edge. It is precisely because of the presence of high-density hydroxyl and carboxyl groups that graphene oxide has good hydrophilicity, is easy to disperse in water, and can form a relatively stable dispersion.
[0004] At the same time, graphene oxide is also a highly promising flame retardant and smoke suppressant filler. Generally, when graphene and its derivatives are added to polymer materials, they can improve the thermal stability of the material, delay the ignition time of the polymer, effectively inhibit the spread of flames, and play a role in controlling the heat release rate and inhibiting the emission of toxic gases. However, when graphene oxide is used alone as a flame retardant filler, the effect is often not ideal. When graphene oxide is used together with other flame retardants or flame retardant elements are introduced into it, a synergistic effect can be achieved.
[0005] In the "graphene oxide composite sponge and its preparation method and application" disclosed in Chinese patent document CN110180514A, a graphene oxide composite sponge and its preparation method and application are disclosed. A clean polyurethane sponge is put into a graphene oxide aqueous solution, and a graphene oxide polyurethane sponge is obtained after drying. Finally, the graphene oxide polyurethane sponge is soaked in an ethanol aqueous solution, and a graphene oxide composite sponge is obtained after a secondary drying treatment. These methods of compounding graphene oxide and polymer foam are simple and convenient to operate, the raw materials are easy to obtain, the time consumption is short, and the environmental pollution is small. However, since graphene oxide is used alone as a flame retardant to be compounded with polyurethane foam, the effect of slowing down the heat release of the composite foam is limited, and it does not have a good effect of inhibiting heat transfer and blocking the overflow of harmful gases during combustion.
[0006] In the Chinese patent document CN114672993A, "A flame-retardant functional cotton fabric based on graphene oxide and its preparation method", the inventors mixed diethylphosphoethyltriethoxysilane, ethanol and deionized water evenly, and stirred vigorously for 12 hours to obtain a mixed solution. Graphene oxide and sandwich polyacid were added to the mixed solution, and ultrasonic treatment was performed for 1 to 3 hours to obtain a flame-retardant finishing solution. The cleaned cotton fabric was padded in the flame-retardant finishing solution, dried and baked in sequence to obtain a graphene oxide flame-retardant cotton fabric. Then it was immersed in hydrazine hydrate for reduction reaction, washed and dried after being taken out to obtain a flame-retardant functional cotton fabric. The flame-retardant functional cotton fabric has the advantages of high safety, good thermal stability, energy saving and environmental protection, and high efficiency flame retardancy. However, this method is complicated and the use of reagents is relatively dangerous.
[0007] In summary, the existing method of using graphene oxide as a flame retardant filler makes it difficult to fill graphene oxide into the interior of polymer foam in a simple and fast way, and it is difficult to take into account both improving the flame retardant and smoke suppression properties of polymer foam materials and improving their thermal insulation and heat preservation properties. In addition, there are generally problems of high cost and low efficiency, and it cannot be widely used in general technical fields. Summary of the invention
[0008] The purpose of the present invention is to provide a method and product for preparing a polymer foam in situ compounded with phosphorus-containing graphene oxide. The present invention has the characteristics of improving the flame retardant, smoke suppression, heat insulation and thermal insulation properties of the polymer foam material, and has the characteristics of simple preparation process and low cost.
[0009] The technical solution of the present invention is a method for preparing a polymer foam by in-situ compounding of phosphorus-containing graphene oxide, comprising the following steps:
[0010] S1. Preparation of phosphorus-containing graphene oxide:
[0011] S101, weighing graphene oxide and a catalyst, adding them to a liquid phosphorus flame retardant, reacting at a temperature of 165 to 215° C. for 12 to 36 hours to obtain a reaction product;
[0012] S102, after centrifugation, the reaction product is washed alternately with deionized water and anhydrous ethanol for 2 to 4 times, and freeze-dried for 24 to 48 hours to obtain dry phosphorus-containing graphene oxide;
[0013] S2. Cleaning polymer foam materials:
[0014] S3, phosphorus-containing graphene oxide is in-situ compounded into the interior of the polymer foam material:
[0015] S301, uniformly dispersing the phosphorus-containing graphene oxide in a solvent by ultrasonication, and obtaining a dispersion after ultrasonication for 0.5 to 5 hours;
[0016] S302, immersing the clean polymer foam into the dispersion, transferring to a vacuum oven for immersion, wherein the vacuum oven temperature is 60 to 90° C., the vacuum degree is 60 to 90 kPa, and the immersion time is 30 to 90 min;
[0017] S303, taking out the polymer foam, keeping it at normal pressure for 12 to 36 hours, transferring the polymer foam to a freeze dryer for freeze drying for 24 to 48 hours, and obtaining a polymer foam in situ compounded with phosphorus-containing graphene oxide.
[0018] In the preparation of the aforementioned phosphorus-containing graphene oxide and its application in polymer foam, in step S101, the catalyst is any one of monobutyltin oxide, dibutyltin oxide, sodium methoxide, potassium hydroxide, sodium hydroxide, potassium tert-butoxide, sulfonic acid, triethylamine, p-toluenesulfonic acid, and 4-dimethylaminopyridine; the liquid phosphorus-based flame retardant is any one of dimethyl methyl phosphate, trimethyl phosphate, dimethyl phosphite, diethyl ethyl phosphate, and diethyl (hydroxymethyl) phosphate, or a mixture of at least two thereof.
[0019] In the preparation of the aforementioned phosphorus-containing graphene oxide and its application in polymer foam, in step S101, the mass ratio of the graphene oxide to the catalyst is (5-15):1; the mass ratio of the graphene oxide to the liquid phosphorus-based flame retardant is 1:(20-60).
[0020] The preparation of the aforementioned phosphorus-containing graphene oxide and its application in polymer foam, in step S2, the polymer foam is any one of polyurethane foam, one-step polyimide foam, melamine foam, silicone foam, polyethylene terephthalate foam, and the open pore degree of the polymer foam is 60 to 100%.
[0021] In the above-mentioned preparation of phosphorus-containing graphene oxide and its application in polymer foam, in step S2, the cleaning method of the polymer foam material is: alternately clean the polymer foam with deionized water and anhydrous ethanol for 2 to 5 times, and after cleaning, place it in an oven at 80 to 100° C. and dry it for 3 to 8 hours to obtain a clean polymer foam.
[0022] In the above-mentioned preparation of phosphorus-containing graphene oxide and its application in polymer foam, in step S301, the solvent used to disperse the phosphorus-containing graphene oxide is any one of deionized water and anhydrous ethanol or a mixture of the two.
[0023] In the aforementioned preparation of phosphorus-containing graphene oxide and its application in polymer foam, in step S301, the concentration of the dispersion is 3 to 20 mg / ml;
[0024] The present solution also includes a phosphorus-containing graphene oxide in-situ composite polymer foam, which is prepared by any of the above-mentioned preparation methods.
[0025] Compared with the uncompounded polymer foam, the aforementioned phosphorus-containing graphene oxide in-situ compounded polymer foam has a limiting oxygen index value increased by 30.0-75.0%, a thermal conductivity value reduced by 20.0-40.0%, an average sound absorption coefficient increased by 110.0-260.0%, and a maximum smoke specific optical density value reduced by 35.0-60.0%.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The present invention selects to first introduce the flame retardant element-phosphorus into the graphene oxide sheet through the reaction sites provided by a large number of oxygen-containing functional groups (such as epoxy groups, hydroxyl groups and carboxyl groups) on the surface and edge of graphene oxide through ester exchange reaction with a liquid phosphorus-based flame retardant, so as to prepare a new type of phosphorus-containing graphene oxide, realize the effective connection between the phosphorus-based flame retardant fragments and the graphene oxide sheet, and prepare a phosphorus / carbon integrated flame retardant functional filler; then the modified graphene oxide containing the flame retardant element phosphorus is used as an inorganic filler, and is precipitated and filled in the polymer foam skeleton (foam flutes and pores) by a vacuum impregnation method. Under the premise of not affecting the pore structure of the foam material itself, the problem of poor flame retardancy, smoke suppression and thermal insulation performance of polymer foams such as polyurethane and one-step polyimide is effectively solved at the same time, and the flame retardancy, smoke suppression, thermal insulation, sound absorption and other properties of the polymer foam are comprehensively improved.
[0028] Compared with uncompounded polymer foam, the obtained phosphorus-containing graphene oxide in-situ compounded polymer foam has a limiting oxygen index value increased by 30.0-75.0%, a thermal conductivity value decreased by 20.0-40.0%, an average sound absorption coefficient increased by 110.0-260.0%, and a maximum smoke specific optical density value decreased by 35.0-60.0%. The present invention successfully prepares a foam material with better comprehensive performance.
[0029] In addition, the preparation process of the present invention is simple, the liquid phosphorus flame retardant required for modification is inexpensive, the overall preparation cost is low, and the safety and efficiency are high. It can effectively solve a series of problems in the previous technical route of using graphene oxide as a flame retardant filler in terms of raw material cost, production time, material commercialization, etc., and provides new ideas and explorations for the future development of high-performance and high-efficiency flame-retardant graphene oxide, and has huge social and economic benefits in practical applications. It is expected to be widely used in ordinary civilian fields relying on its price advantage. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is a photograph of the soft polyurethane foam in-situ compounded with phosphorus-containing graphene oxide prepared in Example 1;
[0031] Figure 2 This is an actual combustion picture of the soft polyurethane foam in-situ compounded with phosphorus-containing graphene oxide prepared in Example 2;
[0032] Figure 3 This is an actual combustion picture of the soft polyurethane foam with graphene oxide in-situ compounding prepared in this comparative example 2;
[0033] Figure 4 It is a performance index diagram of Examples 1-3 and Comparative Examples 1-4. DETAILED DESCRIPTION
[0034] A method for preparing a phosphorus-containing graphene oxide in-situ composite polymer foam comprises the following steps:
[0035] S1. Preparation of phosphorus-containing graphene oxide:
[0036] S101. Weigh graphene oxide and a catalyst, add them to a liquid phosphorus-based flame retardant, react at a temperature of 165 to 215° C. for 12 to 36 hours to obtain a reaction product; wherein the mass ratio of graphene oxide to the catalyst is (5 to 15):1; and the mass ratio of graphene oxide to the liquid phosphorus-based flame retardant is 1:(20 to 60).
[0037] S102, after centrifugation, the reaction product is washed alternately with deionized water and anhydrous ethanol for 2 to 4 times, and freeze-dried for 24 to 48 hours to obtain dry phosphorus-containing graphene oxide;
[0038] The catalyst is any one of monobutyltin oxide, dibutyltin oxide, sodium methoxide, potassium hydroxide, sodium hydroxide, potassium tert-butoxide, sulfonic acid, triethylamine, p-toluenesulfonic acid, and 4-dimethylaminopyridine; the liquid phosphorus flame retardant is any one of dimethyl methyl phosphate, trimethyl phosphate, dimethyl phosphite, diethyl ethyl phosphate, and diethyl (hydroxymethyl) phosphate, or a mixture of at least two of them.
[0039] S2. Cleaning polymer foam materials:
[0040] S201, washing the polymer foam with deionized water and anhydrous ethanol alternately for 2 to 5 times, and after washing, drying it in an oven at 80 to 100° C. for 3 to 8 hours to obtain a clean polymer foam;
[0041] The polymer foam is any one of polyurethane foam, one-step polyimide foam, melamine foam, silicone foam and polyethylene terephthalate foam, and the open pore degree of the polymer foam is 60-100%.
[0042] S3, phosphorus-containing graphene oxide is in-situ compounded into the interior of the polymer foam material:
[0043] S301, uniformly dispersing the phosphorus-containing graphene oxide in a solvent by ultrasonication, and obtaining a dispersion after ultrasonication for 0.5 to 5 hours; wherein the solvent used to disperse the phosphorus-containing graphene oxide is any one of deionized water and anhydrous ethanol or a mixture of the two; and the concentration of the phosphorus-containing graphene oxide dispersion is 3 to 20 mg / ml;
[0044] S302, immersing the clean polymer foam into the dispersion, transferring to a vacuum oven for immersion, wherein the vacuum oven temperature is 60 to 90° C., the vacuum degree is 60 to 90 kPa, and the immersion time is 30 to 90 min;
[0045] S303, taking out the polymer foam, keeping it at normal pressure for 12 to 36 hours, transferring the polymer foam to a freeze dryer for freeze drying for 24 to 48 hours, and obtaining a polymer foam in situ compounded with phosphorus-containing graphene oxide.
[0046] The polymer foam obtained by the in-situ compounding of phosphorus-containing graphene oxide by the preparation method has a limiting oxygen index value increased by 30.0-75.0%, a thermal conductivity value decreased by 20.0-40.0%, an average sound absorption coefficient increased by 110.0-260.0%, and a maximum smoke density value decreased by 35.0-60.0%, compared with the uncompounded polymer foam.
[0047] The present invention is described in detail below through specific examples, but the use and purpose of these exemplary embodiments are only used to list the present invention, and do not constitute any form of limitation on the actual protection scope of the present invention, nor limit the protection scope of the present invention to them.
[0048] Embodiment 1:
[0049] A method for preparing a phosphorus-containing graphene oxide in-situ composite polymer foam comprises the following steps:
[0050] S1. Preparation of phosphorus-containing graphene oxide:
[0051] S101, weighing 5.00 g of graphene oxide and 0.4 g of monobutyltin oxide, adding them to dimethyl methyl phosphate (1.00 mol, 150 g), and reacting at 170° C. for 36 h;
[0052] S102, after the reaction product is centrifuged, it is washed alternately with deionized water and anhydrous ethanol for 3 times, and freeze-dried for 48 hours to obtain dry phosphorus-containing graphene oxide.
[0053] S2. Cleaning polymer foam materials:
[0054] S201. Clean the soft polyurethane foam with an open pore size of 70% with deionized water and anhydrous ethanol alternately for 3 times. After cleaning, place the foam in an oven at 80° C. and dry for 5 hours to obtain a clean soft polyurethane foam.
[0055] S3, phosphorus-containing graphene oxide is in-situ compounded into the interior of the soft polyurethane foam material:
[0056] S301, uniformly dispersing the phosphorus-containing graphene oxide in a solvent having a volume ratio of anhydrous ethanol to deionized water of 1:1 by ultrasonication, and obtaining a dispersion of the phosphorus-containing graphene oxide with a concentration of 5 mg / ml after ultrasonication for 0.5 h;
[0057] S302, immersing the cleaned soft polyurethane foam into the dispersion, and transferring it to a vacuum oven for immersion, wherein the vacuum oven temperature is 60° C., the vacuum degree is 80 kPa, and the immersion time is 30 min;
[0058] S303, taking out the soft polyurethane foam, keeping it at normal pressure for 24 hours, transferring the soft polyurethane foam to a freeze dryer and drying it for 48 hours, and obtaining a soft polyurethane foam in-situ compounded with phosphorus-containing graphene oxide.
[0059] Figure 1 This is a photo of the soft polyurethane foam in-situ compounded with phosphorus-containing graphene oxide prepared in Example 1.
[0060] The properties of the phosphorus-containing graphene oxide in-situ composite soft polyurethane foam prepared in Example 1 are as follows:
[0061] The density of the soft polyurethane foam in situ composited with phosphorus-containing graphene oxide is 14.2 kg / m 3 ; The thermal conductivity value is 0.03471W / (m·K); The limiting oxygen index value is 22.0%; The average sound absorption coefficient is 0.52; The maximum smoke optical density value is 14.55.
[0062] Embodiment 2:
[0063] A method for preparing a phosphorus-containing graphene oxide in-situ composite polymer foam comprises the following steps:
[0064] S1. Preparation of phosphorus-containing graphene oxide:
[0065] S101, weighing 5.00 g of graphene oxide and 0.4 g of monobutyltin oxide, adding them to dimethyl methyl phosphate (1.00 mol, 150 g), and reacting at 170° C. for 36 h;
[0066] S102, after the reaction product is centrifuged, it is washed alternately with deionized water and anhydrous ethanol for 3 times, and freeze-dried for 48 hours to obtain dry phosphorus-containing graphene oxide.
[0067] S2. Cleaning polymer foam materials:
[0068] S201. Clean the soft polyurethane foam with an open pore size of 70% with deionized water and anhydrous ethanol alternately for 3 times. After cleaning, place the foam in an oven at 80° C. and dry it for 5 hours to obtain a clean soft polyurethane foam.
[0069] S3, phosphorus-containing graphene oxide is in-situ compounded into the interior of the soft polyurethane foam material:
[0070] S301, uniformly dispersing the phosphorus-containing graphene oxide in a solvent having a volume ratio of anhydrous ethanol to deionized water of 1:1 by ultrasonication, and obtaining a dispersion of the phosphorus-containing graphene oxide having a concentration of 10 mg / ml after ultrasonication for 0.5 h;
[0071] S302, immersing the cleaned soft polyurethane foam into the dispersion, and transferring it to a vacuum oven for immersion, wherein the vacuum oven temperature is 60° C., the vacuum degree is 80 kPa, and the immersion time is 30 min;
[0072] S303, taking out the soft polyurethane foam, keeping it at normal pressure for 24 hours, transferring the soft polyurethane foam to a freeze dryer and drying it for 48 hours, and obtaining a soft polyurethane foam in-situ compounded with phosphorus-containing graphene oxide.
[0073] The properties of the soft polyurethane foam in-situ compounded with phosphorus-containing graphene oxide prepared in Example 2 are as follows:
[0074] The density of the soft polyurethane foam in situ composited with phosphorus-containing graphene oxide is 19.2 kg / m 3 ; The thermal conductivity value is 0.03128W / (m·K); The limiting oxygen index value is 23.8%; The average sound absorption coefficient is 0.79; The maximum smoke density value is 14.74.
[0075] Figure 2 This is a picture of the actual combustion of the soft polyurethane foam in-situ compounded with phosphorus-containing graphene oxide prepared in Example 2.
[0076] Embodiment 3:
[0077] A method for preparing a phosphorus-containing graphene oxide in-situ composite polymer foam comprises the following steps:
[0078] S1. Preparation of phosphorus-containing graphene oxide:
[0079] S101, weighing 5.00 g of graphene oxide and 0.4 g of monobutyltin oxide, adding them to dimethyl methyl phosphate (1.00 mol, 150 g), and reacting at 170° C. for 36 h;
[0080] S102, after the reaction product is centrifuged, it is washed alternately with deionized water and anhydrous ethanol for 3 times, and freeze-dried for 48 hours to obtain dry phosphorus-containing graphene oxide.
[0081] S2. Cleaning polymer foam materials:
[0082] S201. Clean the soft polyurethane foam with an open pore size of 70% with deionized water and anhydrous ethanol alternately for 3 times. After cleaning, place the foam in an oven at 80° C. and dry it for 5 hours to obtain a clean soft polyurethane foam.
[0083] S3, phosphorus-containing graphene oxide is in-situ compounded into the interior of the soft polyurethane foam material:
[0084] S301, uniformly dispersing the phosphorus-containing graphene oxide in a solvent having an absolute ethanol and deionized water volume ratio of 1:1 by ultrasonication, and obtaining a dispersion having a concentration of 15 mg / ml after ultrasonication for 0.5 h;
[0085] S302, immersing the cleaned soft polyurethane foam into the dispersion, and transferring it to a vacuum oven for immersion, wherein the temperature of the vacuum oven is 60° C., the vacuum degree is 80 kPa, and the immersion time is 30 min;
[0086] S303, taking out the soft polyurethane foam, keeping it at normal pressure for 24 hours, transferring the soft polyurethane foam to a freeze dryer and drying it for 48 hours, and obtaining a soft polyurethane foam in-situ compounded with phosphorus-containing graphene oxide.
[0087] The properties of the phosphorus-containing graphene oxide in-situ composite soft polyurethane foam prepared in Example 3 are as follows:
[0088] The density of the soft polyurethane foam in situ composited with phosphorus-containing graphene oxide is 21.6 kg / m 3 ; The thermal conductivity value is 0.03016W / (m·K); The limiting oxygen index value is 25.6%; The average sound absorption coefficient is 0.68; The maximum smoke density value is 13.36.
[0089] Embodiment 4:
[0090] A method for preparing a phosphorus-containing graphene oxide in-situ composite polymer foam comprises the following steps:
[0091] S1. Preparation of phosphorus-containing graphene oxide:
[0092] S101, weighing 5.00 g of graphene oxide and 0.4 g of monobutyltin oxide, adding them to dimethyl methyl phosphate (1.00 mol, 150 g), and reacting at 170° C. for 36 h;
[0093] S102, after the reaction product is centrifuged, it is washed alternately with deionized water and anhydrous ethanol for 3 times, and freeze-dried for 48 hours to obtain dry phosphorus-containing graphene oxide.
[0094] S2. Cleaning polymer foam materials:
[0095] S201. Clean the soft polyurethane foam with an open pore size of 80% with deionized water and anhydrous ethanol alternately for 3 times. After cleaning, place the foam in an oven at 80° C. and dry it for 5 hours to obtain a clean soft polyurethane foam.
[0096] S3, phosphorus-containing graphene oxide is in-situ compounded into the interior of the soft polyurethane foam material:
[0097] S301, uniformly dispersing the phosphorus-containing graphene oxide in a solvent having an absolute ethanol and deionized water volume ratio of 1:1 by ultrasonication, and obtaining a dispersion having a concentration of 5 mg / ml after ultrasonication for 0.5 h;
[0098] S302, immersing the cleaned soft polyurethane foam into the dispersion, and transferring it to a vacuum oven for immersion, wherein the temperature of the vacuum oven is 60° C., the vacuum degree is 80 kPa, and the immersion time is 30 min;
[0099] S303, taking out the soft polyurethane foam, keeping it at normal pressure for 24 hours, transferring the soft polyurethane foam to a freeze dryer and drying it for 48 hours, and obtaining a soft polyurethane foam in-situ compounded with phosphorus-containing graphene oxide.
[0100] The properties of the soft polyurethane foam in-situ compounded with phosphorus-containing graphene oxide prepared in Example 4 are as follows:
[0101] The density of the soft polyurethane foam in situ composited with phosphorus-containing graphene oxide is 15.1 kg / m 3 ; The thermal conductivity value is 0.03376W / (m·K); The limiting oxygen index value is 24.4%; The average sound absorption coefficient is 0.63; The maximum smoke density value is 13.94.
[0102] Embodiment 5:
[0103] S1. Preparation of phosphorus-containing graphene oxide:
[0104] S101, weighing 5.00 g of graphene oxide and 0.4 g of monobutyltin oxide, adding them to dimethyl methyl phosphate (1.00 mol, 150 g), and reacting at 170° C. for 36 h;
[0105] S102, after the reaction product is centrifuged, it is washed alternately with deionized water and anhydrous ethanol for 3 times, and freeze-dried for 48 hours to obtain dry phosphorus-containing graphene oxide.
[0106] S2. Cleaning polymer foam materials:
[0107] S201. Clean the one-step polyimide foam with an open pore size of 68% three times with deionized water and anhydrous ethanol alternately. After cleaning, place the foam in an oven at 80° C. and dry it for 5 hours to obtain a clean one-step polyimide foam.
[0108] S3, phosphorus-containing graphene oxide is in-situ compounded into the one-step polyimide foam material:
[0109] S301, uniformly dispersing the phosphorus-containing graphene oxide in a solvent having a volume ratio of anhydrous ethanol to deionized water of 1:1 by ultrasonication, and obtaining a dispersion of the phosphorus-containing graphene oxide with a concentration of 5 mg / ml after ultrasonication for 0.5 h;
[0110] S302, immersing the clean one-step polyimide foam into the dispersion, transferring it to a vacuum oven for immersion, the vacuum oven temperature is 60° C., the vacuum degree is 80 kPa, and the immersion time is 30 min;
[0111] S303, taking out the one-step polyimide foam, maintaining it at normal pressure for 24 hours, transferring the one-step polyimide foam to a freeze dryer and drying it for 48 hours, and obtaining the one-step polyimide foam in-situ compounded with phosphorus-containing graphene oxide.
[0112] The properties of the one-step polyimide foam prepared by in-situ compounding of phosphorus-containing graphene oxide in this Example 5 are as follows:
[0113] The density of the soft polyurethane foam in situ composited with phosphorus-containing graphene oxide is 19.8 kg / m 3; The thermal conductivity value is 0.03426W / (m·K); The limiting oxygen index value is 25.3%; The average sound absorption coefficient is 0.67; The maximum smoke density value is 10.05.
[0114] Embodiment 6:
[0115] S1. Preparation of phosphorus-containing graphene oxide:
[0116] S101, weigh 5.00 g of graphene oxide and 0.4 g of monobutyltin oxide, add them to dimethyl phosphite (1.00 mol, 150 g), and react at 165° C. for 36 h;
[0117] S102, after the reaction product is centrifuged, it is washed alternately with deionized water and anhydrous ethanol for 3 times, and freeze-dried for 48 hours to obtain dry phosphorus-containing graphene oxide.
[0118] S2. Cleaning polymer foam materials:
[0119] S201. Clean the soft polyurethane foam with an open pore size of 70% with deionized water and anhydrous ethanol alternately for 3 times. After cleaning, place the foam in an oven at 80° C. and dry it for 5 hours to obtain a clean soft polyurethane foam.
[0120] S3, phosphorus-containing graphene oxide is in-situ compounded into the interior of the soft polyurethane foam material:
[0121] S301, uniformly dispersing the phosphorus-containing graphene oxide in a solvent having a volume ratio of anhydrous ethanol to deionized water of 1:1 by ultrasonication, and obtaining a dispersion of the phosphorus-containing graphene oxide with a concentration of 5 mg / ml after ultrasonication for 0.5 h;
[0122] S302, immersing the cleaned soft polyurethane foam into the dispersion, and transferring it to a vacuum oven for immersion, wherein the temperature of the vacuum oven is 60° C., the vacuum degree is 80 kPa, and the immersion time is 30 min;
[0123] S303, taking out the soft polyurethane foam, keeping it at normal pressure for 24 hours, transferring the soft polyurethane to a freeze dryer and drying it for 48 hours, and obtaining a soft polyurethane foam in-situ compounded with phosphorus-containing graphene oxide.
[0124] The properties of the phosphorus-containing graphene oxide in-situ composite soft polyurethane foam prepared in Example 6 are as follows:
[0125] The density of the soft polyurethane foam in situ composited with phosphorus-containing graphene oxide is 14.6 kg / m 3 ; The thermal conductivity value is 0.03405W / (m·K); The limiting oxygen index value is 21.5%; The average sound absorption coefficient is 0.50; The maximum smoke density value is 14.73.
[0126] Comparative Example 1:
[0127] The soft polyurethane foam with an open pore size of 70% was washed alternately with deionized water and anhydrous ethanol for 3 times, and after being cleaned, it was placed in an oven at 80°C and dried for 5 hours to obtain a clean soft polyurethane foam. Graphene oxide was weighed and uniformly dispersed in a solvent with an anhydrous ethanol and deionized water volume ratio of 1:1 by ultrasonication, and a dispersion was obtained after ultrasonication for 3 hours, and a dispersion with a concentration of 5 mg / ml was obtained.
[0128] The clean soft polyurethane foam is immersed in the dispersion liquid, and transferred to a vacuum oven for immersion at a temperature of 60°C, a vacuum degree of 80 kPa, and an immersion time of 30 minutes. After immersion, the foam is taken out and kept at normal pressure for 24 hours, excess dispersion liquid is removed, and the foam is transferred to a freeze dryer and dried for 48 hours to obtain a soft polyurethane foam with in-situ compounding of graphene oxide.
[0129] The properties of the graphene oxide in-situ composite soft polyurethane foam prepared in Comparative Example 1 are as follows:
[0130] The density of the soft polyurethane foam in situ composited with graphene oxide is 14.6 kg / m 3 ; The thermal conductivity value is 0.03840W / (m·K); The limiting oxygen index value is 19.1%.
[0131] Comparative Example 2:
[0132] The soft polyurethane foam with an open pore size of 70% was washed alternately with deionized water and anhydrous ethanol, and after washing, it was placed in an oven at 80°C for 5 hours to obtain a clean soft polyurethane foam. The graphene oxide was weighed and uniformly dispersed in a solvent with an anhydrous ethanol and deionized water volume ratio of 1:1 by ultrasonication, and a dispersion was obtained after ultrasonication for 3 hours, and a dispersion with a concentration of 10 mg / ml was obtained.
[0133] The clean soft polyurethane foam is immersed in the dispersion liquid, and transferred to a vacuum oven for immersion at a temperature of 60°C, a vacuum degree of 80 kPa, and an immersion time of 30 minutes. After immersion, the foam is taken out and kept at normal pressure for 24 hours, excess dispersion liquid is removed, and the foam is transferred to a freeze dryer and dried for 48 hours to obtain a soft polyurethane foam with in-situ compounding of graphene oxide.
[0134] The properties of the soft polyurethane foam with graphene oxide in-situ compounding prepared in Comparative Example 2 are as follows:
[0135] The density of the soft polyurethane foam with in-situ graphene oxide is 20.2 kg / m 3 ; Thermal conductivity is 0.03793W / (m·K); Limiting oxygen index is 19.8%.
[0136] Figure 3This is an actual combustion picture of the soft polyurethane foam with in-situ compounding of graphene oxide prepared in Comparative Example 2.
[0137] Comparative Example 3:
[0138] The soft polyurethane foam with an open pore size of 70% was washed alternately with deionized water and anhydrous ethanol, and after being cleaned, it was placed in an oven at 80°C and dried for 5 hours to obtain a clean soft polyurethane foam. The graphene oxide was weighed and uniformly dispersed in a solvent with an anhydrous ethanol and deionized water volume ratio of 1:1 by ultrasonication, and a dispersion was obtained after ultrasonication for 3 hours, and a dispersion with a concentration of 15 mg / ml was obtained.
[0139] The clean soft polyurethane foam is immersed in the dispersion liquid, and transferred to a vacuum oven for immersion at a temperature of 60°C, a vacuum degree of 80 kPa, and an immersion time of 30 minutes. After immersion, the foam is taken out and maintained at normal pressure for 24 hours, excess dispersion liquid is removed, and the foam is transferred to a freeze dryer and dried for 48 hours to obtain a soft polyurethane foam with in-situ compounding of graphene oxide.
[0140] The properties of the soft polyurethane foam with graphene oxide in-situ compounding prepared in Comparative Example 3 are as follows:
[0141] The density of the soft polyurethane foam with graphene oxide in situ compounding is 22.2 kg / m 3 ; The thermal conductivity value is 0.03556W / (m·K); The limiting oxygen index value is 20.3%.
[0142] Comparative Example 4:
[0143] The soft polyurethane foam with an open pore size of 70% was cleaned alternately with deionized water and anhydrous ethanol, and after cleaning, it was placed in an oven at 80° C. to dry for 5 hours to obtain a clean soft polyurethane foam.
[0144] The properties of the clean soft polyurethane foam prepared in Comparative Example 4 are as follows:
[0145] The density of clean soft polyurethane foam is 11.6 kg / m 3 ; The thermal conductivity value is 0.04559W / (m·K); The limiting oxygen index value is 16.3%; The average sound absorption coefficient is 0.22; The maximum smoke density value is 24.37.
[0146] Among them, the phosphorus-containing graphene oxide in-situ compounded into the polymer foam in Examples 1-6 is all, and the graphene oxide in-situ compounded into the polymer foam in Comparative Examples 1-3 is. The performance indicators of the samples of Examples 1-6 and Comparative Examples 1-4 are shown in Tables 1 and Figure 4As shown. By observing the limiting oxygen index values and thermal conductivity values of the samples of Examples 1-6 and Comparative Examples 1-4, it is found that the limiting oxygen index values of the samples of Examples 1-6 are higher than those of the samples of Comparative Examples 1-4, and the thermal insulation effect of the samples of Examples 1-6 is better than that of the samples of Comparative Examples 1-4. Therefore, the phosphorus-containing graphene oxide further effectively enhances the flame retardant and thermal insulation properties of the modified polymer foam prepared by using the graphene oxide material as a filler.
[0147] Table 1 Performance of samples of Examples 1-6 and Comparative Examples 1-4
[0148]
Claims
1. A method for preparing a polymer foam by in-situ compounding of phosphorus-containing graphene oxide, characterized in that: The following steps are involved: S1. Preparation of phosphorus-containing graphene oxide: S101, weighing graphene oxide and a catalyst, adding them to a liquid phosphorus flame retardant, reacting at a temperature of 165 to 215° C. for 12 to 36 hours to obtain a reaction product; the liquid phosphorus flame retardant is any one of dimethyl methyl phosphate, trimethyl phosphate, dimethyl phosphite, diethyl ethyl phosphate, and diethyl (hydroxymethyl) phosphate, or a mixture of at least two thereof; S102, after centrifugation, the reaction product is washed alternately with deionized water and anhydrous ethanol, and freeze-dried to obtain dry phosphorus-containing graphene oxide; S2, cleaning the polymer foam material to obtain clean polymer foam; S3, phosphorus-containing graphene oxide is in-situ compounded into the interior of the polymer foam material: S301, uniformly dispersing the phosphorus-containing graphene oxide in a solvent by ultrasonication, and obtaining a dispersion after ultrasonication for 0.5 to 5 hours; S302, immersing the clean polymer foam into the dispersion, transferring to a vacuum oven for immersion, wherein the vacuum oven temperature is 60 to 90° C., the vacuum degree is 60 to 90 kPa, and the immersion time is 30 to 90 min; S303, taking out the polymer foam, maintaining it at normal pressure for 12 to 36 hours, and freeze-drying it for 24 to 48 hours to obtain a polymer foam in-situ compounded with phosphorus-containing graphene oxide.
2. The method for preparing a phosphorus-containing graphene oxide in-situ composite polymer foam according to claim 1, characterized in that: In step S101, the catalyst is any one of monobutyltin oxide, dibutyltin oxide, sodium methoxide, potassium hydroxide, sodium hydroxide, potassium tert-butoxide, sulfonic acid, triethylamine, p-toluenesulfonic acid, and 4-dimethylaminopyridine.
3. The method for preparing a phosphorus-containing graphene oxide in-situ composite polymer foam according to claim 1, characterized in that: In step S101, the mass ratio of graphene oxide to catalyst is (5-15):1; the mass ratio of graphene oxide to liquid phosphorus flame retardant is 1:(20-60).
4. The method for preparing a phosphorus-containing graphene oxide in-situ composite polymer foam according to claim 1, characterized in that: In step S2, the polymer foam is any one of polyurethane foam, one-step polyimide foam, melamine foam, silicone foam, and polyethylene terephthalate foam, and the open pore degree of the polymer foam is 60-100%.
5. The method for preparing a phosphorus-containing graphene oxide in-situ composite polymer foam according to claim 1, characterized in that: In step S2, the polymer foam material is cleaned by alternately cleaning the polymer foam with deionized water and anhydrous ethanol for 2 to 5 times, and after cleaning, placing the polymer foam in an oven at 80 to 100° C. and drying it for 3 to 8 hours to obtain a clean polymer foam.
6. The method for preparing a phosphorus-containing graphene oxide in-situ composite polymer foam according to claim 1, characterized in that: In step S301, the solvent used to disperse the phosphorus-containing graphene oxide is any one of deionized water and anhydrous ethanol or a mixture of the two.
7. The method for preparing a phosphorus-containing graphene oxide in-situ composite polymer foam according to claim 1, characterized in that: In step S301, the concentration of the dispersion is 3-20 mg / ml.
8. A polymer foam in situ compounded with phosphorus-containing graphene oxide, characterized in that: The phosphorus-containing graphene oxide in-situ composite polymer foam is prepared by the preparation method described in any one of claims 1-7.
9. The phosphorus-containing graphene oxide in-situ composite polymer foam according to claim 8, characterized in that: Compared with uncompounded polymer foam, the polymer foam in situ compounded with phosphorus-containing graphene oxide has a limiting oxygen index value increased by 30.0-75.0%, a thermal conductivity value reduced by 20.0-40.0%, an average sound absorption coefficient increased by 110.0-260.0%, and a maximum smoke specific optical density reduced by 35.0-60.0%.
Citation Information
Patent Citations
Graphene oxide composite sponge and preparation method and application thereof
CN110180514A
Flame-retardant functional cotton fabric based on graphene oxide and preparation method of flame-retardant functional cotton fabric
CN114672993A
Preparation method of polymer foam / graphene composite material integrating high heat conductivity and high flexibility
CN105694433A
DOPO derivative flame retardant and preparation and application thereof
CN113956580A
Preparation method and application of polyphosphate grafted graphene flame-retardant modified polypropylene
CN114213759A