A kind of polyester film and preparation method thereof

By using surface-coated glass microbeads as anti-adhesive agent, the impact of silica precipitation in polyester film on electronic devices is solved, and good anti-adhesive performance and stability are achieved, and precipitation in the prior art is avoided. Risk and performance reduction.

CN116444952BActive Publication Date: 2024-11-01SHAOXING XIANGYU GREEN PACKING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310335586.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-11-01
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

There is a risk of precipitation in the addition of amorphous silica in polyester films, which affects the performance of electronic devices, and is difficult to effectively solve the problem in the existing technology.

Method used

Using surface-coated glass microbeads as anti-adhesive agent, a polymethyl methacrylate clad layer is formed by reacting methyl methacrylate, crosslinking agent and initiator to reduce precipitation of silicon elements and improve polyester Compatibility and bonding power of the film.

Benefits of technology

The precipitation of silicon elements is significantly reduced, the anti-adhesion performance of the polyester film and the stability of electronic devices are improved, and the reduction of light transmittance and insufficient surface roughness caused by excessive anti-adhesion agent is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004156320480000051
    Figure BDA0004156320480000051
  • Figure BDA0004156320480000071
    Figure BDA0004156320480000071
Patent Text Reader

Abstract

The present application relates to a polyester film and a preparation method thereof, and relates to the field of polymer materials. The polyester film is prepared by biaxially stretching after blending polyester chips and an anti-sticking agent. The anti-sticking agent is glass microbeads that have been surface-coated, and the particle size of the glass microbeads is 1 to 5 μm; the surface coating layer of the glass microbeads is made of raw materials including the following weight percentages: methyl methacrylate 20 to 35%, solvent 55 to 75%, dispersant 1 to 10%, cross-linking agent 1 to 5%, and initiator 0.1 to 1%. The present application uses polymethyl methacrylate coated glass microbeads as an anti-sticking agent. Compared with amorphous silica powder, the performance of glass microbeads is more stable, and it is not easy to precipitate silicon elements to affect the performance of electronic devices. After the resin coating layer is formed on the surface of the glass microbeads, the glass microbead body is isolated from the outside world, further reducing the effect of silicon element precipitation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of polymer materials, and in particular to a polyester film and a preparation method thereof. Background Art

[0002] Polyester film is made of polyethylene terephthalate as raw material, extruded into thick sheets, and then biaxially stretched to form a film material. Polyester film is a colorless, transparent, glossy film with excellent mechanical properties, high rigidity, hardness and toughness, puncture resistance, friction resistance, high and low temperature resistance, chemical resistance, oil resistance, air tightness and fragrance retention. It is one of the commonly used barrier composite film substrates and is widely used in packaging materials in the fields of food, medicine, textiles, precision instruments, electrical components, etc.

[0003] In the prior art, inorganic silica is generally added to polyester film during the production process. Its function is to increase the roughness of the film surface and play an anti-sticking role, which is beneficial to the unwinding of the polyester film during winding and processing and use to avoid adhesion. The silica commonly used in polyester film is generally in the form of an amorphous powder, and is usually added in the form of a high-concentration masterbatch. However, there is a certain risk of precipitation after amorphous silica is added to polyester film. When polyester film is used in fields such as electronic devices, since electronic devices are mainly made of silicon materials, the precipitation of silicon elements in the polyester film will have a certain impact on the electronic devices. Summary of the invention

[0004] In view of the above technical problems, the present application provides a polyester film and a preparation method thereof, aiming to reduce the influence of the precipitation of anti-sticking agent in the polyester film on electronic devices.

[0005] In a first aspect, the present application provides a polyester film, which adopts the following technical solution:

[0006] A polyester film is prepared by blending polyester chips and an anti-sticking agent, wherein the anti-sticking agent is glass microbeads that have been surface-coated, and the particle size of the glass microbeads is 1-5 μm; the surface coating layer of the glass microbeads is made of raw materials including the following weight percentages: 20-35% of methyl methacrylate, 55-75% of a solvent, 1-10% of a dispersant, 1-5% of a cross-linking agent, and 0.1-1% of an initiator.

[0007] By adopting the above technical solution, the performance of glass microbeads is more stable than that of amorphous silica micropowders, and it is not easy to precipitate silicon elements to affect the performance of electronic devices. On this basis, the glass microbeads are surface coated. Methyl methacrylate will form polymethyl methacrylate during the reaction with the crosslinking agent and the initiator, and then coated on the surface of the glass microbeads to obtain glass microbeads with polymethyl methacrylate surface coating. After the resin coating layer is formed on the surface of the glass microbeads, the glass microbead body is isolated from the outside world, further reducing the precipitation of silicon elements. In addition, the glass microbeads after surface coating have better compatibility with the polyester film raw material, can be well dispersed in the polyester film and have a strong bonding force with the polyester material, and have a good anti-sticking effect.

[0008] Optionally, the anti-adhesive agent is prepared by the following method:

[0009] S1, dispersing methyl methacrylate, dispersant and cross-linking agent in a solvent, heating to 60-80°C, and keeping the temperature for 1-2h to obtain an emulsion;

[0010] S2, mixing the surface-modified glass microspheres with the initiator, heating to 80-90°C, keeping the temperature for reaction for 3-5h, adding the emulsion in step S1, stirring and reacting at 70-80°C for 1-2h;

[0011] S3, filtering to remove the liquid, and drying to obtain an anti-sticking agent.

[0012] By adopting the above technical solution, after the surface modification of the glass microspheres, activated groups appear on the surface, and the hydrophilic surface is changed into a lipophilic surface, and the resin material can be well attached and coated on the surface. After the surface-modified glass microspheres are mixed with the initiator, a grafting reaction can occur, so that the initiator is attached to the surface of the glass microspheres. In the subsequent mixing reaction with the emulsion, the polymerization reaction of the emulsion in methyl methacrylate is initiated more on the surface of the glass microspheres, and the polymethyl methacrylate obtained by polymerization is coated on the surface of the glass microspheres to form a stable coating layer.

[0013] Optionally, the glass microspheres are surface modified by:

[0014] S1. Treat the glass beads in a sodium hydroxide solution for 1 to 2 hours, filter, wash, and dry;

[0015] S2. Mix the coupling agent and glass microbeads, raise the temperature to 50-60° C. for reaction for 1-2 hours, and obtain surface-modified glass microbeads after drying.

[0016] Optionally, the coupling agent is aminopropyltrimethoxysilane or aminopropyltriethoxysilane.

[0017] Optionally, the coupling agent accounts for 2-5% of the mass percentage of the glass microspheres.

[0018] By adopting the above technical scheme, a large number of exposed active groups can be generated on the surface of the glass microbeads after the glass microbeads react in the alkaline solution, and the exposed silanol groups on the surface of the glass microbeads undergo a grafting reaction with the coupling agent molecules to obtain glass microbeads coated with the coupling agent. After the initiator is mixed with the glass microbeads, it will further react with the coupling agent, and then the initiator molecules are first coated on the surface of the glass microbeads to initiate the polymerization reaction of methyl methacrylate on the surface of the glass microbeads, thereby forming a stable coating layer on the surface of the glass microbeads.

[0019] Optionally, the initiator is dibenzoyl peroxide.

[0020] Optionally, the cross-linking agent is a mixture of one or more of ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, and trimethylolpropane triacrylate.

[0021] Optionally, the dispersant is polyethylene glycol.

[0022] Optionally, the solvent is ethanol.

[0023] Optionally, the mass ratio of the anti-sticking agent to the polyester chips is 0.5-2%.

[0024] By adopting the above technical solution, using too much anti-sticking agent will reduce the light transmittance of the polyester film and affect its use, while adding too little anti-sticking agent will not make the surface of the polyester film rough enough, resulting in poor anti-sticking performance.

[0025] Optionally, the mass ratio of the raw material of the surface coating layer to the glass microspheres is (1-5):100.

[0026] By adopting the above technical solution, when coating the glass microbeads, it is necessary to ensure that the resin material completely covers the surface of the glass microbeads to isolate the surface of the glass microbeads from contact with the polyester film raw material. If the amount of the raw material of the coating layer is too small, the thickness of the coating layer will be too thin, which is prone to surface defects; and if the amount of the raw material of the coating layer is too large, the thickness of the coating layer will be too thick, affecting the stability of the performance of the anti-sticking agent.

[0027] In a second aspect, the present application provides a method for preparing a polyester film, using the following technical solution:

[0028] A method for preparing a polyester film comprises the following steps:

[0029] S1, taking polyester chips, drying them, mixing and dispersing them with anti-adhesive agents, and then melt-extruding them;

[0030] S2, the extruded material is cast, biaxially stretched, shaped, cooled and then rolled up to obtain a polyester film.

[0031] Optionally, the intrinsic viscosity of the polyester chips is 0.7.

[0032] Optionally, the temperature of melt extrusion in step S2 is 250-280°C.

[0033] Optionally, the shaping temperature in step S2 is 210-230°C.

[0034] Optionally, during the biaxial stretching process in step S2, the longitudinal stretching ratio is 3.0 to 4.0, and the transverse stretching ratio is 3.5 to 5.0.

[0035] By adopting the above technical solution, the polyester chips and the anti-adhesive agent can be well fused during the melt extrusion process after being mixed and dispersed, and the anti-adhesive agent can be evenly dispersed in the polyester film, so that the roughness of the polyester film surface is improved to achieve a good anti-adhesive effect. The glass microbeads coated with polymethyl methacrylate have good compatibility with the polyester chip melt, which is conducive to the uniform mixing and dispersion of the anti-adhesive agent and the polyester chips. Selecting polyester chips with a characteristic viscosity slightly higher than that of general fiber polyester chips will make the polyester film more tough during the stretching process and less prone to problems such as breakage.

[0036] In summary, the present application includes at least one of the following beneficial technical effects:

[0037] 1. In the technical solution of the present application, polymethyl methacrylate-coated glass microspheres are used as anti-sticking agents. Compared with amorphous silica powder, the performance of glass microspheres is more stable and it is not easy to precipitate silicon elements to affect the performance of electronic devices. After the resin coating layer is formed on the surface of the glass microspheres, the glass microspheres are isolated from the outside world, further reducing the precipitation of silicon elements. In addition, the glass microspheres after surface coating have better compatibility with the raw materials of the polyester film, can be well dispersed in the polyester film and have a strong bonding force with the polyester material, thereby achieving a good anti-sticking effect.

[0038] 2. In the technical solution of the present application, after the surface modification treatment, activated groups appear on the surface of the glass microspheres, and the hydrophilic surface becomes a lipophilic surface, and the resin material can be well attached and coated on the surface. The surface-modified glass microspheres can undergo a grafting reaction after being mixed with an initiator, so that the initiator is attached to the surface of the glass microspheres. In the subsequent mixing reaction with the emulsion, the polymerization reaction of the emulsion in methyl methacrylate is initiated more on the surface of the glass microspheres, and the polymethyl methacrylate obtained by polymerization is coated on the surface of the glass microspheres to form a stable coating layer.

[0039] 3. In the technical solution of the present application, the glass microbeads are subjected to surface modification treatment before surface coating. After the glass microbeads react in alkaline solution, a large number of exposed active groups can be generated on the surface of the glass microbeads. The exposed silanol groups on the surface of the glass microbeads undergo a grafting reaction with the coupling agent molecules to obtain glass microbeads coated with the coupling agent. After the initiator is mixed with the glass microbeads, it will further react with the coupling agent, and then the initiator molecules are first coated on the surface of the glass microbeads to initiate the polymerization reaction of methyl methacrylate on the surface of the glass microbeads, thereby forming a stable coating layer on the surface of the glass microbeads. DETAILED DESCRIPTION

[0040] The present application is further described in detail below in conjunction with specific examples. It should be noted that, if no specific conditions are specified in the following examples, all are carried out under conventional conditions or conditions recommended by the manufacturer; the raw materials used in the following examples can be obtained from common commercial sources unless otherwise specified.

[0041] Preparation example of modified glass microspheres

[0042] Preparation Example 1

[0043] S1. Take solid glass microbeads with an average particle size of 3 μm, immerse them in a 10% sodium hydroxide solution, stir and react for 2 hours, filter out the alkali solution, wash with a deionized beam to remove the alkali solution, and dry to remove moisture;

[0044] S2. The glass microspheres treated with alkali solution were mixed with aminopropyltrimethoxysilane in a mass ratio of 50:1, and the mixture was heated to 50° C. and stirred for reaction for 2 h. The mixture was dried at 110° C. to obtain modified glass microspheres.

[0045] Preparation Example 2

[0046] The difference between this preparation example and preparation example 1 is that the mass ratio of glass microspheres to aminopropyltrimethoxysilane is 20:1, and the rest is consistent with preparation example 1.

[0047] Preparation Example 3

[0048] The difference between this preparation example and preparation example 1 is that the mass ratio of glass microspheres to aminopropyltrimethoxysilane is 100:1, and the rest is consistent with preparation example 1.

[0049] Preparation Example 4

[0050] The difference between this preparation example and preparation example 1 is that the glass microspheres are not treated with alkali solution, and the rest are consistent with preparation example 1.

[0051] Preparation Example 5

[0052] The difference between this preparation example and preparation example 1 is that the glass microspheres are not modified by coupling agent, and the rest are consistent with preparation example 1.

[0053] Preparation Example of Anti-adhesive Agent

[0054] Preparation Example 6

[0055] S1. Referring to the ratio in Table 1, methyl methacrylate, polyethylene glycol and ethylene glycol dimethacrylate were dispersed in ethanol, heated to 60 degrees Celsius and stirred for 2 hours to prepare an emulsion;

[0056] S2. Take the modified glass microspheres prepared in Preparation Example 1 and mix them with dibenzoyl peroxide, keep them warm at 80° C. for 3 hours, add the emulsion prepared in step S1, keep them warm at 70° C. for 2 hours with stirring, then filter to remove the liquid, and dry them at 110° C. to prepare an anti-sticking agent.

[0057] Preparation Example 7

[0058] The difference between this preparation example and preparation example 6 is that the proportion of raw material components is different, please refer to Table 1 for details, and the rest is consistent with preparation example 6.

[0059] Preparation Example 8

[0060] The difference between this preparation example and preparation example 6 is that the proportion of raw material components is different, please refer to Table 1 for details, and the rest is consistent with preparation example 6.

[0061] Preparation Example 9

[0062] The difference between this preparation example and preparation example 6 is that the proportion of raw material components is different, please refer to Table 1 for details, and the rest is consistent with preparation example 6.

[0063] Table 1: Ratio of raw material components in preparation examples 6 to 9 (kg)

[0064]

[0065] Preparation Example 10

[0066] The difference between this preparation example and preparation example 8 is that the anti-sticking agent is prepared by preparation example 2, and the rest is consistent with preparation example 8.

[0067] Preparation Example 11

[0068] The difference between this preparation example and preparation example 8 is that the anti-sticking agent is prepared by preparation example 3, and the rest is consistent with preparation example 8.

[0069] Preparation Example 12

[0070] The difference between this preparation example and preparation example 8 is that the anti-sticking agent is prepared by preparation example 4, and the rest is consistent with preparation example 8.

[0071] Preparation Example 13

[0072] The difference between this preparation example and preparation example 8 is that the anti-sticking agent is prepared by preparation example 5, and the rest is consistent with preparation example 8.

[0073] Preparation Example 14

[0074] The difference between this preparation example and preparation example 8 is that the initiator is added to the emulsion. The specific preparation method is as follows:

[0075] S1, dispersing methyl methacrylate, polyethylene glycol and ethylene glycol dimethacrylate in ethanol, heating to 60 degrees Celsius and stirring for 2 hours, then adding dibenzoyl peroxide and stirring and mixing to form an emulsion;

[0076] S2. Mix the modified glass microbeads prepared in Preparation Example 1 with the emulsion prepared in step S1, stir and react at 70° C. for 2 h, filter to remove the liquid, and dry at 110° C. to prepare an anti-sticking agent.

[0077] The rest are consistent with Preparation Example 8.

[0078] Example 1

[0079] A polyester film, the raw materials include polyester chips and anti-sticking agent, the anti-sticking agent accounts for 0.5% of the polyester chips by mass, the anti-sticking agent is prepared by Preparation Example 6, and the specific preparation method is as follows:

[0080] S1, taking polyester chips with an intrinsic viscosity of 0.7, drying and removing moisture, mixing and dispersing with an anti-sticking agent, and then putting them into a twin-screw extruder, and melt-extrude at 260° C. to obtain an extrudate;

[0081] S2. After the extrudate is cast into a sheet, it is first stretched longitudinally with a longitudinal stretching ratio of 3.0, and then stretched transversely with a transverse stretching ratio of 3.5. After stretching, it is shaped at 210°C, cooled, and rolled up to obtain a polyester film; the thickness of the polyester film is 30±2μm.

[0082] Example 2

[0083] The difference between this embodiment and embodiment 1 is that the anti-sticking agent is prepared by Preparation Example 7, and the rest is consistent with embodiment 1.

[0084] Example 3

[0085] The difference between this embodiment and embodiment 1 is that the anti-sticking agent is prepared by Preparation Example 8, and the rest is consistent with embodiment 1.

[0086] Example 4

[0087] The difference between this embodiment and embodiment 1 is that the anti-sticking agent is prepared by Preparation Example 9, and the rest is consistent with embodiment 1.

[0088] Example 5

[0089] The difference between this embodiment and embodiment 1 is that the anti-sticking agent is prepared by Preparation Example 10, and the rest is consistent with embodiment 1.

[0090] Example 6

[0091] The difference between this embodiment and embodiment 1 is that the anti-sticking agent is prepared by Preparation Example 11, and the rest is consistent with embodiment 1.

[0092] Example 7

[0093] The difference between this embodiment and embodiment 1 is that the anti-sticking agent is prepared by Preparation Example 12, and the rest is consistent with embodiment 1.

[0094] Example 8

[0095] The difference between this embodiment and embodiment 1 is that the anti-sticking agent is prepared by Preparation Example 13, and the rest is consistent with embodiment 1.

[0096] Example 9

[0097] The difference between this embodiment and embodiment 1 is that the anti-sticking agent is prepared by Preparation Example 14, and the rest is consistent with embodiment 1.

[0098] Comparative Example 1

[0099] The difference between Comparative Example 1 and Example 1 is that an equal amount of glass microspheres with an average particle size of 3 μm is used instead of the anti-sticking agent, and the rest is consistent with Example 1.

[0100] Performance testing

[0101] The polyester films prepared in the above examples and comparative examples were tested for their properties. The test results are shown in Table 2 below.

[0102] Table 2: Performance test results of Examples 1 to 8 and Comparative Example 1

[0103]

[0104] It can be seen from the data in Table 2 that the polyester film made by using glass microbeads with surface coating instead of silicon dioxide as an anti-adhesive agent has good anti-adhesive properties, and the strength and optical properties of the polyester film are not lower than those of the polyester film made with silicon dioxide as an anti-adhesive agent. By surface coating silicon dioxide, the glass microbeads are isolated from the polyester material, which can effectively avoid the precipitation of silicon element during use. It can be seen from the test data that the silicon content test value is significantly reduced.

[0105] In addition, by further surface modification of the glass microspheres and adjusting the parameters of the modification, the compatibility between the anti-sticking agent made of the glass microspheres and the polyester material can be further improved, thereby improving the strength of the polyester film.

[0106] It can be seen from the data of Example 9 that in the process of surface coating of glass microbeads, by first grafting the initiator onto the surface of the glass microbeads, it is easier to form a film on the surface of the glass microbeads in the subsequent emulsion polymerization coating process to coat the glass microbeads and form a stable coating layer. When the initiator is directly mixed in the emulsion, the coating effect of the emulsion on the surface of the glass microbeads will deteriorate to a certain extent, resulting in a decrease in the strength of the polyester film and a significant increase in the detected value of the silicon content.

[0107] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A polyester film, characterized in that The polyester chips and the anti-adhesive agent are blended and then biaxially stretched to obtain the anti-adhesive agent, which is glass microbeads that have been surface-coated, and the particle size of the glass microbeads is 1-5 μm; the surface coating layer of the glass microbeads is made of the following raw materials in weight percentage: methyl methacrylate 20-35%, solvent 55-75%, dispersant 1-10%, cross-linking agent 1-5%, initiator 0.1-1%; The anti-adhesive agent is prepared by the following method: S1, dispersing methyl methacrylate, dispersant and cross-linking agent in a solvent, heating to 60-80°C, and keeping the temperature for 1-2h to obtain an emulsion; S2, mixing the surface-modified glass microspheres with the initiator, heating to 80-90°C, keeping the temperature for reaction for 3-5h, adding the emulsion in step S1, stirring and reacting at 70-80°C for 1-2h; S3, filtering to remove the liquid, and drying to obtain an anti-sticking agent; The glass microspheres are surface modified by the following method: S1. Treat the glass beads in a sodium hydroxide solution for 1-2 hours, filter, wash and dry; S2, mixing the coupling agent with the glass microbeads, heating to 50-60°C for reaction for 1-2h, and drying to obtain the surface-modified glass microbeads; The mass ratio of the raw material of the surface coating layer to the glass microspheres is 1:2, 1:4.5 or 1:

10.

2. A polyester film according to claim 1, characterized in that: The coupling agent is aminopropyltrimethoxysilane or aminopropyltriethoxysilane.

3. A polyester film according to claim 1, characterized in that: The coupling agent accounts for 2-5% of the mass of the glass microspheres.

4. A polyester film according to claim 1, characterized in that: The initiator is dibenzoyl peroxide.

5. A polyester film according to claim 1, characterized in that: The mass ratio of the anti-sticking agent to the polyester chips is 0.5-2%.

6. The method for preparing a polyester film according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1, taking polyester chips, drying them, mixing and dispersing them with anti-adhesive agents, and then melt-extruding them; S2, the extruded material is cast, biaxially stretched, shaped, cooled and then rolled up to obtain a polyester film.

7. The method for preparing a polyester film according to claim 6, characterized in that: The intrinsic viscosity of the polyester chips is 0.7.