A hydrophobic coating for photovoltaic modules and preparation method thereof
By using surface-modified hydrophobic coatings composed of perlite, acrylic and xylene, the problems of pollutant accumulation and frame corrosion in photovoltaic modules are solved, and the components are self-cleaned and efficiently generated, reducing costs and improving Tolerability.
Patent Information
- Application Number
- CN202310509457.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-05-08
AI Technical Summary
The hydrophobic coatings of existing photovoltaic modules are costly, have low environmental tolerance and low mechanical strength in applications, making it difficult to effectively prevent pollutant accumulation and aluminum frame corrosion, affecting the power generation efficiency and reliability of the module.
Using surface-modified hydrophobic coating composed of grinding perlite, acrylic resin and xylene, the hydrophobic properties of the coating are improved and water can pass quickly through the irregular sheet structure of grinding perlite and the use of surface modifiers. The surface of the component takes away contaminants to avoid frame corrosion.
The self-cleaning effect of photovoltaic modules is achieved, the light transmittance and power generation efficiency is improved, the service life of the module is extended, while reducing costs and improving environmental tolerance.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention belongs to the field of coatings, and in particular relates to a hydrophobic coating for a photovoltaic module and a preparation method thereof. Background Art
[0002] When photovoltaic modules work outdoors for a long time, pollutants such as dust and rain will accumulate on the glass surface of the modules, causing heating of the modules, reduced light transmittance, reduced power and other problems. At the same time, seawater and acid rain will corrode the aluminum frame of the modules, seriously affecting the reliability of the modules. Therefore, a coating with self-cleaning ability that allows water to pass through the modules quickly will greatly improve the power generation efficiency and reliability of photovoltaic modules. When water passes through the modules quickly, it will take away most of the dust and other pollutants, while avoiding corrosion of the aluminum frame. There are currently two technical solutions: hydrophobic coating and super hydrophilic coating. However, such coatings are currently rarely used in the photovoltaic field, and most of them are high in cost, low in environmental tolerance, and low in mechanical strength. Summary of the invention
[0003] In view of the problems existing in the prior art, the present invention provides a hydrophobic coating with high hydrophobicity and self-cleaning effect. When water falls on a photovoltaic module coated with the hydrophobic coating of the present invention, it can quickly pass through the surface of the module, while taking away pollutants such as dust on the surface of the module, achieving the effect of self-cleaning of the module, improving the light transmittance of the surface glass, avoiding heating of the module battery due to pollutants, thereby improving the efficiency and reliability of the module; in addition, in seawater or acid rain environments, water quickly passes through the frame of the module, avoiding frame corrosion, and improving the long-term reliability of the photovoltaic module.
[0004] Specifically, the first aspect of the present invention provides a hydrophobic coating for photovoltaic modules, wherein the hydrophobic coating comprises surface-modified ground perlite, acrylic resin and xylene, wherein the surface-modified ground perlite is ground perlite whose surface is modified by polymethylhydrogensiloxane and / or silanol fluid, the particle size of the ground perlite is 10-30 microns, and the ground perlite has an irregular flaky structure.
[0005] In one or more embodiments, based on 100 parts by weight of the total weight of the components of the hydrophobic coating except the surface modifier, the mass of the ground perlite in the hydrophobic coating is 5-95 parts by weight.
[0006] In one or more embodiments, the ground perlite is obtained by grinding hollow spherical perlite.
[0007] In one or more embodiments, the hollow spherical perlite has a particle size of 100-500 microns.
[0008] In one or more embodiments, the hollow spherical perlite is expanded perlite.
[0009] In one or more embodiments, based on 100 parts by weight of the total weight of the components of the hydrophobic coating except the surface modifier, the mass of the surface modifier in the hydrophobic coating is 0.05-5 parts by weight.
[0010] In one or more embodiments, the surfactant is polymethylhydrogensiloxane.
[0011] In one or more embodiments, in the hydrophobic coating, the mass of the polymethylhydrogensiloxane is 0.5%-1.5% of the mass of the ground perlite.
[0012] In one or more embodiments, the surfactant is a silanol fluid.
[0013] In one or more embodiments, the mass of the silanol fluid in the hydrophobic coating is 3% to 7% of the mass of the ground perlite.
[0014] In one or more embodiments, the acrylic resin is selected from one or more of isobutyl methacrylate / styrene resin, butyl acrylate resin, methacrylate resin, methyl methacrylate resin, and methyl methacrylate / styrene resin.
[0015] In one or more embodiments, based on 100 parts by weight of the total weight of the components of the hydrophobic coating except the surface modifier, the mass of the acrylic resin in the hydrophobic coating is 1-20 parts by weight.
[0016] In one or more embodiments, the xylene is selected from one or more of meta-xylene, para-xylene, and ortho-xylene.
[0017] In one or more embodiments, the xylene is a mixture of meta-xylene, para-xylene, and ortho-xylene.
[0018] In one or more embodiments, the xylene is composed of 45% to 70% by mass of meta-xylene, 15% to 25% by mass of para-xylene, and 10% to 15% by mass of o-xylene.
[0019] In one or more embodiments, based on 100 parts by weight of the total weight of the components of the hydrophobic coating except the surface modifier, the mass of the xylene in the hydrophobic coating is 3-80 parts by weight.
[0020] In one or more embodiments, the hydrophobic coating consists of surface modified ground perlite, acrylic resin, and xylene.
[0021] A second aspect of the present invention provides a method for preparing a hydrophobic coating as described in any embodiment herein, the method comprising the following steps:
[0022] (1) grinding the hollow spherical perlite to obtain ground perlite;
[0023] (2) uniformly dispersing the surface modifier and the ground perlite in water, and then drying to remove water to obtain the surface-modified perlite; and
[0024] (3) The acrylic resin and the xylene are mixed evenly, the surface-modified perlite is added to the mixture of the acrylic resin and the xylene, the mixture is mixed evenly, and then coated on the glass surface to obtain the hydrophobic coating.
[0025] In one or more embodiments, in the step (3), the coating has a thickness of 0.5-1 mm. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The contact angle variation curves of the coatings of Examples 1-7 at different filler ratios.
[0027] Figure 2 The contact angle (A) and rolling angle (B) curves of the coating of Example 2 at different soaking times.
[0028] Figure 3 The contact angle and coating weight (A) and rolling angle (B) of the coating of Example 2 are changed with the friction intensity (sand weight). The dark diamonds represent the angles, the light squares represent the coating weight, and the coating weight refers to the mass percentage of the coating to the total weight of the coating and the glass.
[0029] Figure 4 This is a photograph of the coating of Example 2 under an optical microscope.
[0030] Figure 5 This is a photo of the coating of Example 2 taken under an electron microscope.
[0031] Figure 6 The contact angle variation curves of the coatings of Examples 8-17 at different filler ratios.
[0032] Figure 7 The contact angle (A) and rolling angle (B) curves of the coating of Example 11 at different soaking time are shown.
[0033] Figure 8 The contact angle and coating weight (A) and rolling angle (B) of the coating of Example 11 are changed with the friction intensity (weight of sand). The dark diamonds represent the angles, the light squares represent the coating weight, and the coating weight refers to the mass percentage of the coating to the total weight of the coating and the glass.
[0034] Fig. 9 This is a photograph of the coating of Example 11 under an optical microscope.
[0035] Fig.10 This is a photograph of the coating of Example 11 under an electron microscope.
[0036] Fig.11 : is an optical microscope photograph of the expanded perlite before grinding in Examples 1-17.
[0037] Fig.12 : is an optical microscope photograph of the ground perlite in Example 1-17.
[0038] Fig.13 This is the particle size analysis of the expanded perlite before grinding in Examples 1-17.
[0039] Fig.14 The particle size analysis of the perlite after grinding in Examples 1-17. DETAILED DESCRIPTION
[0040] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0041] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0042] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.
[0043] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0044] Herein, unless otherwise specified, percentage refers to mass percentage, ratio refers to mass ratio, and part refers to mass part.
[0045] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.
[0046] Herein, the sum of the percentages of the various components of the composition is 100%.
[0047] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0048] The inventors found that the use of surface modifiers to modify ground perlite to prepare a hydrophobic coating can make the coating have a larger contact angle and a smaller rolling angle when in contact with water, and has good hydrophobic properties. For example, in some preferred embodiments, the contact angle of the coating of the present invention in contact with water is more than 130°, even up to about 150°, and the rolling angle is below 10°, or even below 5°. When water falls on a photovoltaic module, it can quickly pass through the surface of the module, while taking away pollutants such as dust on the surface, achieving self-cleaning of the module, improving the surface transmittance, and avoiding heating of the module battery due to pollutants, thereby improving the efficiency and reliability of the module. In addition, in seawater or acid rain environments, water can also quickly pass through the frame of the module to avoid frame corrosion and improve the long-term reliability of the photovoltaic module. Therefore, the present invention provides a hydrophobic coating for a photovoltaic module, the hydrophobic coating comprising surface-modified ground perlite, acrylic resin and xylene.
[0049] In the present invention, ground perlite refers to ground perlite. The particle size of the ground perlite is preferably 10-30 microns, such as 15 microns, 20 microns, and 25 microns. The ground perlite suitable for the present invention has an irregular flaky structure. The use of perlite with a particle size of 10-30 microns and an irregular flaky structure is beneficial to improving the hydrophobic properties of the coating.
[0050] In the present invention, the perlite used for grinding is preferably hollow spherical perlite, such as expanded perlite. The main components and mass fractions of expanded perlite are shown in Table 1 below. The particle size of the hollow spherical perlite (such as expanded perlite) can be 100-500 microns.
[0051] Table 1: Main components of expanded perlite (unit: wt%)
[0052] type <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> <![CDATA[Fe 2 THE 3 ]]> CaO <![CDATA[K 2 The]]> <![CDATA[Na 2 The]]> MgO <![CDATA[H 2 The]]> Perlite 68~74 11~13 0.5~3.6 0.7~1.0 2~3 4~5 0.3 2.3~6.4
[0053] The spatial structure of the ground perlite is an irregular flaky structure, which is arranged in parallel, vertical or intersecting manner, and the particle size is 10-30 microns, for example, about 20 microns. Since the ground perlite is an irregular flaky structure, the internal space of the coating of the present invention is composed of an irregular flaky structure or parallel, vertical or intersecting. The irregular flaky structure and irregular spatial arrangement result in a micron and submicron rough structure on the surface of the coating, providing a base material for the hydrophobic coating. The rough structure will greatly increase the gas-solid surface, and when water falls on the coating surface, the air will lift the water droplets, thereby achieving a high contact angle and a high rolling angle.
[0054] In the hydrophobic coating of the present invention, the total weight of the components of the hydrophobic coating except the surface modifier is 100 parts by mass, and the mass of perlite is 5-95 parts by mass, such as 10 parts by mass, 20 parts by mass, 30 parts by mass, 40 parts by mass, 50 parts by mass, 60 parts by mass, 65 parts by mass, 70 parts by mass, 75 parts by mass, 80 parts by mass, 85 parts by mass, 90 parts by mass. In the present invention, unless otherwise specified, the mass fraction of a certain component in the hydrophobic coating is 100 parts by mass relative to the total weight of the components of the hydrophobic coating except the surface modifier. When the ratio of grinding perlite in the coating is higher (such as grinding perlite mass fraction ≥ 60 parts by mass), this micron and submicron rough structure will be greatly increased, not only the rough structure on the same plane increases, but each layer in the coating is the structure, and the hydrophobicity and wear resistance of the coating are greatly improved.
[0055] The method of grinding the hollow spherical perlite is not particularly limited, as long as the ground perlite with the desired particle size and irregular flake structure can be obtained, for example, grinding can be performed using a grinder.
[0056] The surface modifier of the present invention should be a surface modifier with good film-forming properties. Preferably, the surface modifier is selected from polymethyl hydrogen siloxane and / or silanol fluid, which is conducive to improving the hydrophobic coating of the coating. In the hydrophobic coating of the present invention, the total weight of the components of the hydrophobic coating except the surface modifier is 100 parts by mass, and the mass of the surface modifier can be 0.05-5 parts by mass, such as 0.1 parts by mass, 0.5 parts by mass, 1 parts by mass, and 2 parts by mass. The specific content of the surface modifier is adjusted according to the amount of ground perlite. When the surface modifier is polymethyl hydrogen siloxane, the mass of polymethyl hydrogen siloxane in the hydrophobic coating is preferably 0.5%-1.5% of the mass of perlite, such as 1%. When the surface modifier is a silanol fluid, the mass of silanol in the hydrophobic coating is preferably 3%-7% of the mass of ground perlite, such as 4%, 5%, and 6%. Controlling the content of the surface modifier within the aforementioned range is conducive to improving the hydrophobic properties of the coating.
[0057] Generally, the surface modifier can be added to the ground perlite, water is used as a solvent to fully dissolve the surface modifier and the ground perlite and mix them evenly, and the modified ground perlite is obtained after drying to completely evaporate the water. The surface modifier used in the present invention has an active chemical bond in its molecular structure, which can react with the silicon dioxide in the perlite in the coating system to reduce the surface energy of the system, thereby improving the hydrophobicity of the coating.
[0058] The acrylic resin suitable for the present invention can be selected from one or more of isobutyl methacrylate / styrene resin, butyl acrylate resin, methacrylate resin, methyl methacrylate resin and methyl methacrylate / styrene resin. Among them, isobutyl methacrylate / styrene resin is a transparent, non-toxic thermoplastic resin with good processing fluidity, weather resistance, impact strength, low hygroscopicity, excellent optical properties and light transmittance. The use of the above acrylic resin can better protect the hydrophobic base layer in the coating system.
[0059] In the hydrophobic coating of the present invention, based on 100 parts by weight of the total weight of the components of the hydrophobic coating excluding the surface modifier, the mass of the acrylic resin can be 1-20 parts by weight, for example, 2 parts by weight, 5 parts by weight, 10 parts by weight, or 15 parts by weight.
[0060] Xylene is a colorless, transparent, and fluid liquid. The xylene suitable for the present invention can be selected from one or more of meta-xylene, para-xylene, or o-xylene. Preferably, the xylene used in the present invention is a mixture of the above three xylene isomers, which is conducive to improving the hydrophobic properties of the coating. In some preferred embodiments, the xylene is composed of 45%-70% by mass of meta-xylene, 15%-25% by mass of para-xylene, and 10%-15% by mass of o-xylene. Using xylene as a solvent for acrylic resin in the system can fully dissolve the acrylic resin and allow it to be fully mixed with the ground perlite.
[0061] In the hydrophobic coating of the present invention, based on the total weight of the components of the hydrophobic coating excluding the surface modifier as 100 parts by mass, the mass of xylene can be 3-80 parts by mass, for example, 10 parts by mass, 20 parts by mass, 30 parts by mass, 40 parts by mass, 50 parts by mass, 60 parts by mass, or 70 parts by mass.
[0062] In some embodiments, based on 100 parts by weight of the total weight of the components of the hydrophobic coating excluding the surface modifier, the hydrophobic coating contains:
[0063] Ground perlite, 5-95 parts by mass,
[0064] Surface modifier, 0.05-5 parts by mass,
[0065] Xylene, 3-80 parts by mass, and
[0066] Acrylic resin, 1-20 parts by mass.
[0067] The hydrophobic coating of the present invention can be prepared by a method comprising the following steps:
[0068] (1) grinding the hollow spherical perlite to obtain ground perlite;
[0069] (2) uniformly dispersing the surface modifier and the ground perlite in water, and then drying to remove water to obtain surface-modified perlite; and
[0070] (3) The acrylic resin and xylene are mixed evenly, the surface-modified perlite is added to the mixture of the acrylic resin and xylene, the mixture is mixed evenly, and then coated on the glass surface to obtain the hydrophobic coating of the present invention.
[0071] In step (3), the coating thickness may be 0.5-1 mm.
[0072] The present invention has the following beneficial effects:
[0073] The present invention can make photovoltaic modules achieve self-cleaning effect, improve the light transmittance of the module surface, avoid frame corrosion, and improve module efficiency and long-term reliability. At the same time, the hydrophobic coating of the present invention has a simple formula, low cost, strong hydrophobicity, and high environmental tolerance.
[0074] The present invention will be further described in the following by way of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The expanded perlite used in the present invention was purchased from Xinyang Juncheng Mining Co., Ltd. The xylene in the examples is composed of 65% by mass of m-xylene, 20% by mass of p-xylene and 15% by mass of o-xylene. The isobutyl methacrylate / styrene resin in the examples is Unless otherwise specified, the methods and reagents used in the examples are conventional methods and reagents in the art.
[0075] Example 1
[0076] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 0.85 parts by mass of polymethylhydrogensiloxane is added to 85 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the polymethylhydrogensiloxane and the ground perlite. Put it into a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. Add 3 parts by mass of isobutyl methacrylate / styrene resin to 12 parts by mass of xylene, mix it thoroughly and dissolve it. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix it thoroughly and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0077] Example 2
[0078] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 0.75 parts by mass of polymethylhydrogensiloxane is added to 75 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the polymethylhydrogensiloxane and the ground perlite. Put it into a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. Add 5 parts by mass of isobutyl methacrylate / styrene resin to 20 parts by mass of xylene, mix it thoroughly and dissolve it. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix it thoroughly and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0079] Example 3
[0080] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 0.65 parts by mass of polymethylhydrogensiloxane is added to 65 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the polymethylhydrogensiloxane and the ground perlite. Put it into a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. Add 7 parts by mass of isobutyl methacrylate / styrene resin to 28 parts by mass of xylene, mix it thoroughly and dissolve it. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix it thoroughly and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0081] Example 4
[0082] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 0.55 parts by mass of polymethylhydrogensiloxane is added to 55 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the polymethylhydrogensiloxane and the ground perlite. Put it into a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. 9 parts by mass of isobutyl methacrylate / styrene resin is added to 36 parts by mass of xylene, and it is fully mixed and dissolved. The modified ground perlite is added to the mixture of isobutyl methacrylate / styrene resin and xylene, and after it is fully mixed and dissolved, it is applied to the glass surface with a thickness of 0.5 mm.
[0083] Example 5
[0084] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 0.45 parts by mass of polymethylhydrogensiloxane is added to 45 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the polymethylhydrogensiloxane and the ground perlite. Put it into a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. Add 11 parts by mass of isobutyl methacrylate / styrene resin to 44 parts by mass of xylene, mix it thoroughly and dissolve it. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix it thoroughly and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0085] Example 6
[0086] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 0.35 parts by mass of polymethylhydrogensiloxane is added to 35 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the polymethylhydrogensiloxane and the ground perlite. Put it into a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. Add 13 parts by mass of isobutyl methacrylate / styrene resin to 52 parts by mass of xylene, mix it thoroughly and dissolve it. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix it thoroughly and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0087] Example 7
[0088] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 0.25 parts by mass of polymethylhydrogensiloxane is added to 25 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the polymethylhydrogensiloxane and the ground perlite. Put it into a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. Add 15 parts by mass of isobutyl methacrylate / styrene resin to 60 parts by mass of xylene, mix it thoroughly and dissolve it. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix it thoroughly and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0089] Example 8
[0090] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 4.75 parts by mass of silanol fluid is added to 95 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the silanol fluid and the ground perlite. Place it in a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. Add 1 part by mass of isobutyl methacrylate / styrene resin to 4 parts by mass of xylene, mix it thoroughly and dissolve it. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix it thoroughly and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0091] Example 9
[0092] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 4.25 parts by mass of silanol fluid is added to 85 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the silanol fluid and the ground perlite. Put it into a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. Add 3 parts by mass of isobutyl methacrylate / styrene resin to 12 parts by mass of xylene, mix it thoroughly and dissolve it. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix it thoroughly and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0093] Example 10
[0094] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 3.75 parts by mass of silanol fluid is added to 75 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the silanol fluid and the ground perlite. Put it into a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. Add 5 parts by mass of isobutyl methacrylate / styrene resin to 20 parts by mass of xylene, mix it thoroughly and dissolve it. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix it thoroughly and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0095] Embodiment 11
[0096] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 3.25 parts by mass of silanol fluid is added to 65 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the silanol fluid and the ground perlite. Put it into a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. Add 7 parts by mass of isobutyl methacrylate / styrene resin to 28 parts by mass of xylene, mix it thoroughly and dissolve it. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix it thoroughly and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0097] Example 12
[0098] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 2.75 parts by mass of silanol fluid is added to 55 parts by mass of ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the silanol fluid and ground perlite. Put it into a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. 9 parts by mass of isobutyl methacrylate / styrene resin is added to 36 parts by mass of xylene, and it is fully mixed and dissolved. The modified ground perlite is added to the mixture of isobutyl methacrylate / styrene resin and xylene, and after it is fully mixed and dissolved, it is applied to the glass surface with a thickness of 0.5 mm.
[0099] Embodiment 13
[0100] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 2.25 parts by mass of silanol fluid is added to 45 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the silanol fluid and the ground perlite. Place it in a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. Add 11 parts by mass of isobutyl methacrylate / styrene resin to 44 parts by mass of xylene, mix it thoroughly and dissolve it. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix it thoroughly and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0101] Embodiment 14
[0102] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 1.75 parts by mass of silanol fluid is added to 35 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the silanol fluid and the ground perlite. Place it in a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. 13 parts by mass of isobutyl methacrylate / styrene resin is added to 52 parts by mass of xylene, and it is fully mixed and dissolved. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0103] Embodiment 15
[0104] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 1.25 parts by mass of silanol fluid is added to 25 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the silanol fluid and the ground perlite. Put it into a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. Add 15 parts by mass of isobutyl methacrylate / styrene resin to 60 parts by mass of xylene, mix it thoroughly and dissolve it. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix it thoroughly and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0105] Example 16
[0106] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 0.75 parts by mass of silanol fluid is added to 15 parts by mass of the ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the silanol fluid and the ground perlite. Place it in a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. 17 parts by mass of isobutyl methacrylate / styrene resin is added to 68 parts by mass of xylene, and it is fully mixed and dissolved. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0107] Embodiment 17
[0108] After the expanded perlite is ground to a particle size of 20 microns with a grinder, 0.25 parts by mass of silanol fluid is added to 5 parts by mass of ground perlite, and ultrapure water is used as a solvent to fully dissolve and mix the silanol fluid and ground perlite. Place it in a drying chamber to completely evaporate the water, and the sample becomes completely dried modified ground perlite. 19 parts by mass of isobutyl methacrylate / styrene resin is added to 76 parts by mass of xylene, and it is fully mixed and dissolved. Add the modified ground perlite to the mixture of isobutyl methacrylate / styrene resin and xylene, mix and dissolve it, and then apply it to the glass surface with a thickness of 0.5 mm.
[0109] Comparative Example 1
[0110] Add 0.75 parts by mass of polymethyl hydrogen siloxane to 75 parts by mass of silicon dioxide with a particle size of 20 microns, and use ultrapure water as a solvent to fully dissolve and mix the polymethyl hydrogen siloxane and silicon dioxide. Place in a drying chamber to completely evaporate the water, and the sample becomes completely dried modified silicon dioxide. Add 5 parts by mass of isobutyl methacrylate / styrene resin to 20 parts by mass of xylene, mix and dissolve them thoroughly. Add the modified silicon dioxide to the mixture of isobutyl methacrylate / styrene resin and xylene, mix and dissolve them thoroughly, and then apply it to the glass surface with a thickness of 0.5 mm.
[0111] Comparative Example 2
[0112] Add 3.25 parts by mass of silanol fluid to 65 parts by mass of silicon dioxide with a particle size of 20 microns, use ultrapure water as solvent, and fully dissolve and mix the silanol fluid and silicon dioxide. Put it into a drying chamber to completely evaporate the water, and the sample becomes completely dry modified silicon dioxide. Add 7 parts by mass of isobutyl methacrylate / styrene resin to 28 parts by mass of xylene, mix it thoroughly and dissolve it. Add the modified silicon dioxide to the mixture of isobutyl methacrylate / styrene resin and xylene, mix it thoroughly and dissolve it, and then apply it to the glass surface with a thickness of 0.5mm.
[0113] The raw materials and amounts used in each embodiment and comparative example are shown in Table 2 below.
[0114] Table 2: Raw materials and amounts in Examples and Comparative Examples (unit: parts by mass, based on the total weight of the components of the hydrophobic coating excluding the surface modifier as 100 parts by mass)
[0115]
[0116] Note: “ / ” means not added.
[0117] Performance parameter detection
[0118] The various parameters and properties of the hydrophobic coatings prepared in Examples 1-17 and Comparative Examples 1-2 were tested, including the contact angle, the rolling angle, and the curve of the contact angle changing with the friction intensity. The contact angle and the rolling angle were measured in accordance with the standard ASTM F21-20. The mechanical properties test method of the coating is as follows: the glass coated with the coating is placed and fixed at 45° to the horizontal, and sand with a particle size of 0.5-1 mm of different weights is dropped from a height of 1.5 m each time to rub the coating; the contact angle and the rolling angle are recorded before and after each friction test. The waterproof performance test method is as follows: the glass coated with the coating is placed in water with a depth of 10 cm and soaked for different lengths of time, and the contact angle and the rolling angle are recorded before and after each soaking test.
[0119] The test results of contact angle and rolling angle are as follows: Figure 1 , Figure 6 The results show that when modified with polymethylhydrogensiloxane, the coating of Example 2 in Examples 1-7 has the largest contact angle and the best hydrophobicity (e.g. Figure 1 ); In addition, the rolling angle of the coating in Example 2 is 3°. When the coating surface is 3° to the horizontal, water droplets can quickly pass through the coating surface; when modified with silanol fluid, the coating contact angle of Example 11 in Examples 8-17 is the largest and the hydrophobicity is the best under different filler ratios (such as Figure 6 ); the rolling angle of Example 11 is also 3°, and water droplets can quickly pass through the coating surface. Compared with Example 2, except for the different grinding of perlite and silica, the other coating preparation conditions are the same, and the coating contact angle of Comparative Example 1 is 121°, the rolling angle is 15°, and the hydrophobicity is general. The hydrophobic performance of the coating of Example 2 is significantly better than that of the coating of Comparative Example 1. Compared with Example 11, except for the different grinding of perlite and silica, the other coating preparation conditions are the same; and the coating contact angle of Comparative Example 2 is 117°, the rolling angle is 18°, and the hydrophobicity is general; the hydrophobic performance of the coating of Example 11 is significantly better than that of the coating of Comparative Example 2.
[0120] Table 3: Contact angle and sliding angle of coatings in Examples and Comparative Examples
[0121]
[0122]
[0123] Further testing of the various properties of the coatings in Example 2 and Example 11, the results of the mechanical properties and waterproof properties of the coatings are as follows: Figure 1-14 As shown. Figure 2 As shown in FIG. 1 , as the soaking time increases, the contact angle of the coating in Example 2 first decreases and then returns to the original level (eg Figure 2(A)); At the same time, the rolling angle is kept at 3-5° during the soaking process (such as Figure 2 (B)), indicating that the coating of Example 2 has good waterproof performance. Figure 3 As shown in FIG. 1 , as the friction intensity increases, the contact angle of the coating in Example 2 first increases and then begins to decrease, and then remains at about 130° (as shown in FIG. 1 ). Figure 3 (A)); while the roll angle is kept between 3-7° (such as Figure 3 (B)), indicating that the coating of Example 2 has excellent mechanical properties. Figure 4 As shown, the coating in Example 2 has a rough structure under an optical microscope, which will greatly increase the air-solid surface. When water falls on the coating surface, the air will lift the water droplets, thereby achieving a high contact angle and a high rolling angle. Figure 5 As shown, the coating in Example 2 is a micron or submicron structure under an electron microscope, and is composed of irregular flaky structures that are either parallel, vertical, or intersecting, thereby resulting in a submicron rough structure on the coating surface.
[0124] like Figure 7 As shown, as the soaking time of the coating in Example 11 increases, the contact angle of the coating first decreases and then returns to the original level (eg Figure 7 (A)); At the same time, during this process, the rolling angle is always maintained at 2-5° (such as Figure 7 (B)), indicating that the coating of Example 11 has good waterproof performance. Figure 8 As shown in FIG. 1 , as the friction intensity increases, the contact angle of the coating in Example 11 first increases and then begins to decrease, and then remains at about 119° (as shown in FIG. 11 ). Figure 8 (A)), while the roll angle is kept between 2-6° (e.g. Figure 8 (B)), the coating has excellent mechanical properties. Fig. 9 As shown in FIG. 11 , the coating surface of Example 11 is a rough structure under an optical microscope, which will greatly increase the air-solid surface. When water falls on the coating surface, the air will lift the water droplets, thereby achieving a high contact angle and a high rolling angle. Fig.10 As shown, the coating of Example 11 is a micron or submicron structure under an electron microscope, and is composed of irregular flaky structures that are either parallel, vertical, or intersecting, thereby resulting in a submicron rough structure on the coating surface.
[0125] Overall, Example 2 and Example 11 have the best technical effects.
[0126] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A hydrophobic coating for a photovoltaic module, characterized in that: The hydrophobic coating comprises surface-modified ground perlite, acrylic resin and xylene, wherein the surface-modified ground perlite is ground perlite whose surface is modified by polymethylhydrogensiloxane and / or silanol fluid; The ground perlite is obtained by grinding hollow spherical perlite, the particle size of the hollow spherical perlite is 100-500 microns, the particle size of the ground perlite is 10-30 microns, and the ground perlite has an irregular flaky structure; Wherein, based on the total weight of the components of the hydrophobic coating except the surface modifier being 100 parts by weight, the mass of the ground perlite in the hydrophobic coating is 65-95 parts by weight.
2. The hydrophobic coating according to claim 1, characterized in that Based on 100 parts by weight of the total weight of the components of the hydrophobic coating except the surface modifier, the mass of the ground perlite in the hydrophobic coating is 75-95 parts by weight.
3. The hydrophobic coating according to claim 1, characterized in that The hollow spherical perlite is expanded perlite.
4. The hydrophobic coating according to claim 1, characterized in that Based on the total weight of the components of the hydrophobic coating except the surface modifier being 100 parts by weight, the mass of the surface modifier in the hydrophobic coating is 0.05-5 parts by weight.
5. The hydrophobic coating according to claim 1, characterized in that The surface modifier is polymethylhydrogensiloxane.
6. The hydrophobic coating according to claim 5, characterized in that In the hydrophobic coating, the mass of the polymethylhydrogensiloxane is 0.5%-1.5% of the mass of the ground perlite.
7. The hydrophobic coating according to claim 1, characterized in that The surface modifier is a silanol fluid.
8. The hydrophobic coating according to claim 7, characterized in that In the hydrophobic coating, the mass of the silanol fluid is 3%-7% of the mass of the ground perlite.
9. The hydrophobic coating according to claim 1, characterized in that The acrylic resin is selected from one or more of isobutyl methacrylate / styrene resin, butyl acrylate resin, methacrylate resin, methyl methacrylate resin and methyl methacrylate / styrene resin.
10. The hydrophobic coating according to claim 1, characterized in that Based on 100 parts by weight of the total weight of the components of the hydrophobic coating except the surface modifier, the mass of the acrylic resin in the hydrophobic coating is 1-20 parts by weight.
11. The hydrophobic coating according to claim 1, wherein The xylene is selected from one or more of meta-xylene, para-xylene and o-xylene.
12. The hydrophobic coating according to claim 11, characterized in that The xylene is a mixture of meta-xylene, para-xylene and o-xylene.
13. The hydrophobic coating according to claim 11 or 12, characterized in that: The xylene is composed of 45% to 70% by mass of m-xylene, 15% to 25% by mass of p-xylene and 10% to 15% by mass of o-xylene.
14. The hydrophobic coating according to claim 1, wherein Based on 100 parts by weight of the total weight of the components of the hydrophobic coating except the surface modifier, the weight of the xylene in the hydrophobic coating is 3-80 parts by weight.
15. The hydrophobic coating according to claim 1, wherein The hydrophobic coating consists of surface-modified ground perlite, acrylic resin and xylene.
16. A method for preparing a hydrophobic coating according to any one of claims 1 to 15, characterized in that: The method comprises the following steps: (1) grinding the hollow spherical perlite to obtain ground perlite; (2) uniformly dispersing the surface modifier and the ground perlite in water, and then drying to remove water to obtain the surface-modified perlite; and (3) The acrylic resin and the xylene are mixed evenly, the surface-modified perlite is added to the mixture of the acrylic resin and the xylene, the mixture is mixed evenly, and then coated on the glass surface to obtain the hydrophobic coating.
17. The method according to claim 16, characterized in that In the step (3), the coating thickness is 0.5-1 mm.