A method for preparing wafer-level single crystals based on the directional growth of two-dimensional transition metal chalcogenide single crystals under an electric field environment.

By controlling the growth of crystal nuclei and regulating the electric field strength under an electric field environment, the problems of random domain orientation and high grain boundary density in two-dimensional transition metal chalcogenide single crystals have been solved, enabling the controllable preparation of large-size wafer-level single crystals and reducing production difficulty and cost.

CN116446034BActive Publication Date: 2026-11-10ZHENGZHOU UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310270894.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2026-11-10
Estimated Expiration
2043-03-20

AI Technical Summary

Technical Problem

Existing chemical vapor deposition methods for preparing two-dimensional transition metal chalcogenide single crystals suffer from problems such as random domain orientation, small single crystal size, high grain boundary density, and multilayer stacking, which lead to high production difficulty and cost, thus limiting their industrial application.

Method used

The growth of crystal nuclei is controlled under an electric field environment. By adjusting the concentration of the metal oxometalate solution and the intensity of the external electric field, the directional growth of crystal nuclei is ensured, and seamless splicing is achieved to form large-size wafer-level single crystals.

Benefits of technology

The directional growth of single crystals of two-dimensional transition metal chalcogenides has been achieved, solving the problems of random domain orientation and high grain boundary density, reducing production difficulty and cost, and making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004134599670000011
    Figure HDA0004134599670000011
  • Figure HDA0004134599670000012
    Figure HDA0004134599670000012
  • Figure HDA0004134599670000013
    Figure HDA0004134599670000013
Patent Text Reader

Abstract

This invention discloses a method for preparing wafer-level single crystals of two-dimensional transition metal chalcogenides (TMCs) under an electric field environment. A metal oxoate solution is uniformly coated onto a SiO2 / Si silicon wafer substrate. The silicon wafer substrate is then placed in the first high-temperature zone of a tube furnace, and sulfur powder or selenium powder is placed in the second high-temperature zone. A growth carrier gas is continuously introduced into the quartz tube of the tube furnace, and the reaction takes place under the atmosphere of the growth carrier gas. The power switch of the flat-plate electric field is turned on, and the voltage is adjusted to maintain a constant electric field strength. The first high-temperature zone is heated for growth, while the second high-temperature zone is simultaneously heated and kept at a constant temperature. After completion, the growth carrier gas is continuously introduced until the temperature drops to room temperature, yielding the product: a two-dimensional wafer-level TMC single crystal. This invention solves the problems of random domain orientation, small single crystal size, and high multilayer stacking and grain boundary density in the two-dimensional TMC process, avoiding special requirements for the growth substrate and reducing production costs and process difficulty.
Need to check novelty before this filing date? Find Prior Art

Description

I. Technical Field:

[0001] This invention relates to the highly directional growth of two-dimensional transition metal chalcogenide single crystals and the technology for preparing large-size wafer-level single crystals, belonging to the field of two-dimensional nanomaterial production technology, specifically relating to a method for preparing wafer-level single crystals based on the directional growth of two-dimensional transition metal chalcogenide single crystals under an electric field environment. II. Background Technology:

[0002] Two-dimensional transition metal chalcogenides (TMCs) are layered semiconductor materials with excellent thermal and chemical stability. In 2005, physicist Novoselov mechanically disrupted the van der Waals forces between the layers of MoS2, exfoliating a monolayer of MoS2 and thus initiating research on TMCs. TMCs exhibit a typical "sandwich" structure. Taking MoS2 as an example, it consists of two layers of sulfur (S) atoms sandwiching a layer of mo (Mo) atoms (S-Mo-S), with the Mo and S atoms linked by covalent bonds. The monolayer of a TMC possesses an intrinsically suitable band gap. In transistor fabrication, using an insulating oxide layer as the dielectric layer significantly increases the mobility of the monolayer two-dimensional atomic material at room temperature. As the integration density of electronic devices increases, the size of traditional silicon-based transistors is approaching physical limits, posing a significant challenge to the continuation of Moore's Law. TMCs, with their suitable band gap and high carrier mobility, have become essential core materials for continuing Moore's Law and driving the development of modern integrated circuits.

[0003] With the continuous in-depth research on two-dimensional transition metal chalcogenide materials, various production and preparation methods have been reported. Among them, chemical vapor deposition (CVD) exhibits significant advantages due to its simple operation, low operating cost, and numerous adjustable parameters. Furthermore, in the production and preparation of other related two-dimensional materials, CVD has achieved controllable preparation of nanoscale graphene single-crystal films and wafer-level hexagonal boron nitride single-crystal films. However, the preparation of two-dimensional wafer-level transition metal chalcogenide single crystals places particularly stringent requirements on the growth substrate, necessitating the construction of nanoscale steps on the substrate surface. This extremely high level of process expertise significantly increases the difficulty and cost of preparing two-dimensional transition metal chalcogenide wafer-level single crystals.

[0004] Meanwhile, the synthesis of two-dimensional transition metal chalcogenide (TMC) wafer-level single crystals using chemical vapor deposition (CVD) suffers from problems such as small single crystal size, random growth orientation, high grain boundary density, and multilayer crystal stacking, which greatly limit its industrial application. The main reason is that during CVD, TMC forms multiple crystal nuclei on the substrate surface in the early stages of growth. As the reaction progresses, these nuclei grow into small single crystals with random growth directions. Furthermore, these small single crystals can grow further and merge with adjacent single crystals. Due to their different crystal growth orientations, grain boundaries form during merging, preventing the formation of a grain boundary-free thin film. Grain boundaries, which are typically highly reactive, become new nuclei, leading to the formation of new small single crystals above them. This easily results in double or multilayer stacking structures, ultimately leading to high internal grain boundary density, poor mechanical properties, and uncontrollable layer number in the resulting two-dimensional TMC crystalline thin film. Moreover, electron transport within the two-dimensional material is hindered by these grain boundaries, significantly limiting the integration and industrialization of TMC semiconductor devices. Therefore, it is particularly important to solve problems such as random orientation of single crystals, grain boundaries, and size during the growth of two-dimensional transition metal chalcogenides. III. Summary of the Invention:

[0005] The technical problem to be solved by this invention is: in order to overcome the problems of random domain orientation, small single crystal size, multilayer stacking and high grain boundary density in the production of two-dimensional transition metal chalcogenides by existing chemical vapor deposition methods, and to avoid special requirements on the growth substrate, reduce production costs and process difficulty, this invention provides a method for preparing wafer-level single crystals based on the directional growth of two-dimensional transition metal chalcogenides single crystals under an electric field environment.

[0006] To solve the above problems, the technical solution adopted by the present invention is as follows:

[0007] This invention provides a method for preparing wafer-level single crystals by directional growth of two-dimensional transition metal chalcogenide single crystals under an electric field environment. The preparation method includes the following steps:

[0008] a. Add metal oxophosphate powder to deionized water to prepare a solution with a concentration of 0.001–0.05 mol / L;

[0009] b. The metal oxophosphate solution obtained in step a is dropped onto the hydrophilically treated SiO2 / Si silicon wafer substrate, and the solution is evenly distributed on the silicon wafer substrate using a spin coater;

[0010] c. Place the silicon wafer substrate coated with metal oxoate solution in step b into the first high-temperature zone of the tube furnace, and place sulfur powder or selenium powder into the second high-temperature zone upstream. The amount of sulfur powder added is 50-500 mg, and the amount of selenium powder added is 50-500 mg.

[0011] d. Remove impurity gases from the atmosphere of the quartz tube in the tubular furnace by introducing argon gas with a purity of 99.999% at a flow rate of 300-600 sccm to remove other gases in the quartz tube for 10-20 minutes; during the reaction, argon gas or an argon-hydrogen mixture is continuously introduced as the growth carrier gas.

[0012] e. Turn on the power switch of the flat plate electric field and adjust the voltage to maintain a constant electric field strength in the flat plate electric field;

[0013] f. The first high-temperature zone in step c is heated at a first heating rate to a reaction growth temperature of 750-900°C for growth, and the growth time is 3-10 min. At the same time, the second high-temperature zone is heated at a second heating rate to a set temperature of 150-350°C for a constant temperature time of 3-20 min.

[0014] g. After the reaction growth is completed, argon or argon-hydrogen mixture as described in step d is continuously introduced until the temperature drops to room temperature. Then, the argon or argon-hydrogen mixture and the flat electric field power supply are turned off to obtain the product, a two-dimensional wafer-level transition metal chalcogenide single crystal.

[0015] According to the above-described method for preparing wafer-level single crystals by directional growth of two-dimensional transition metal chalcogenide single crystals under an electric field environment, the metal oxoate in step a is any one of Na2MoO4, Na3VO4, Na2WO4, and NaNbO3; the particle size of the metal oxoate powder is ≤2μm.

[0016] According to the above-described method for preparing wafer-level single crystals by directional growth of two-dimensional transition metal chalcogenide single crystals under an electric field environment, the rotation speed of the spin coater in step b is 500-5000 r / min, and the holding time is 30-120 s.

[0017] According to the above-described method for preparing wafer-level single crystals by directional growth of two-dimensional transition metal chalcogenide single crystals under an electric field environment, the distance between the first high-temperature region and the second high-temperature region in step c is 15-20 cm.

[0018] According to the above method for preparing wafer-level single crystals by directional growth of two-dimensional transition metal chalcogenide single crystals under an electric field environment, the flow rate of argon or argon-hydrogen mixture as the growth carrier gas in step d is 100-300 sccm, and the proportion of hydrogen in the argon-hydrogen mixture is 1-10%.

[0019] According to the above-described method for preparing wafer-level single crystals by directional growth of two-dimensional transition metal chalcogenide single crystals under an electric field environment, the electric field strength in step e is 100–500 V / cm.

[0020] According to the above-described method for preparing wafer-level single crystals by directional growth of two-dimensional transition metal chalcogenide single crystals under an electric field environment, the first heating rate in step f is 10-20℃ / min, and the second heating rate is 5-40℃ / min.

[0021] The technical solution of this invention first spin-coates a metal oxoate solution onto a SiO2 / Si silicon wafer substrate that has undergone hydrophilic treatment. Then, by controlling the growth temperature, carrier gas flow rate, and other conditions, crystal nuclei are formed on the substrate surface. The number and density of crystal nuclei on the silicon wafer substrate surface are controlled by controlling the concentration and hydrophilicity of the metal oxoate solution. At the same time, the growth orientation of the transition metal chalcogenide crystal is controlled under the regulation of an external electric field, so that the directional growth becomes a two-dimensional transition metal chalcogenide wafer-level single crystal with the same crystal domain orientation. By controlling the concentration of the metal oxoate solution, small single crystals with the same crystal domain orientation are driven to form a wafer-level single crystal without grain boundaries.

[0022] The positive and beneficial effects of this invention are:

[0023] 1. Compared with the prior art, the technical solution of the present invention utilizes the effect of an electric field on metal ions to regulate the growth orientation of two-dimensional single crystal wafers, thus solving the problem of random growth orientation of two-dimensional transition metal chalcogenide crystals in the traditional vapor deposition method.

[0024] 2. The technical solution of this invention utilizes the strategy of controlling crystal orientation by electric field and achieves seamless splicing growth, which solves the problems of small size and high grain boundary density of current two-dimensional transition metal chalcogenide single crystals, and is expected to realize the controllable preparation of large-size wafer-level single crystals.

[0025] 3. The preparation method of this invention ensures consistent crystal domain orientation among small grains during growth, enabling them to be assembled into wafer-level single crystals during the reaction process. Furthermore, this method has low equipment requirements, avoids the need for special growth substrates, and has a simple operation process. Therefore, it can be considered an ideal method for the industrial production of two-dimensional transition metal chalcogenide wafer-level single crystals. IV. Description of the attached drawings:

[0026] Figure 1 A schematic diagram of the apparatus for preparing wafer-level single crystals by directional growth of two-dimensional transition metal chalcogenides;

[0027] Figure 2 Optical image of MoS2 prepared in Example 1 of this invention;

[0028] Figure 3Raman spectrum of monolayer MoS2 prepared in Example 1 of this invention;

[0029] Figure 4 Photoluminescence spectrum of monolayer MoS2 prepared in Example 1 of this invention;

[0030] Figure 5 Monolayer height diagram of the monolayer MoS2 prepared in Example 1 of this invention;

[0031] Figure 6 STEM image of the atomic structure of monolayer MoS2 prepared in Example 1 of this invention;

[0032] Figure 7 A photograph of the wafer-level MoS2 single crystal prepared in Example 1 of this invention;

[0033] Figure 8 Optical microscope image of WS2 prepared in Example 3 of this invention;

[0034] Figure 9 An optical microscope image of randomly distributed MoS2 prepared in Example 5 of this invention.

[0035] Figure 1 This is a schematic diagram of the apparatus for preparing wafer-level single crystals by directional growth of two-dimensional transition metal chalcogenide single crystals according to the present invention. The two-dimensional transition metal chalcogenide single crystals are driven to grow in a highly directional manner by adding an additional electric field. Figure 2 and Figure 8 These are optical microscope images of the unidirectionally aligned MoS2 and WS2 cells prepared in Example 1 of this invention. Figure 2 and Figure 8 As can be seen, the triangular MoS2 and WS2 grown by the technique of this invention have the same direction, while the growth direction of MoS2 grown by conventional vapor deposition is random (as shown in the attached figure). Figure 9 As shown in the figure, the electric field modulation has a good effect on the growth orientation control of two-dimensional MoS2 single crystals and shows a single alignment direction. Further Raman spectroscopy, photoluminescence and height tests on the MoS2 prepared in Example 1 of this invention all show that the prepared MoS2 is a single-layer structure.

[0036] in, Figure 3 The Raman spectrum of MoS2 prepared in Example 1 of this invention shows typical characteristic peaks of molybdenum disulfide, where molybdenum disulfide A... 1g and E 2g The difference is 20cm -1 The prepared molybdenum disulfide has a single-layer structure. Furthermore, Figure 4 The photoluminescence spectrum of MoS2 prepared in Example 1 of this invention, and Figure 5This is a height diagram of the single-layer MoS2 prepared in Example 1 of the present invention. The thickness of the prepared MoS2 is approximately 0.82 nm, further demonstrating that the prepared molybdenum disulfide is a single-layer structure. Similar results were obtained by testing under the same conditions in other locations on this wafer-level single-crystal thin film, proving the uniformity of the obtained film. Meanwhile, Figure 6 The image shows a STEM image of MoS2 obtained in this invention, proving that the atomic structure of MoS2 is complete and there are no grain boundaries. Figure 7 This is a photograph of the wafer-level MoS2 single crystal prepared according to the present invention; it shows the wafer-level crystal size and also illustrates the uniformity of the wafer-level thin film. V. Detailed Implementation Methods:

[0037] The present invention will be further illustrated below with reference to the embodiments, but this does not limit the scope of protection of the technical solution of the present invention.

[0038] Example 1:

[0039] The detailed steps of the method for preparing two-dimensional MoS2 single crystals with a single growth orientation according to the present invention are as follows:

[0040] a. Place 1.030g of analytical grade sodium molybdate (Na2MoO4) powder into a 100mL volumetric flask and dilute to volume with deionized water to prepare a solution with a concentration of 0.01mol / L.

[0041] b. The sodium molybdate solution obtained in step a is dropped onto a 1×1cm SiO2 / Si silicon wafer substrate that has undergone hydrophilic treatment, and the silicon wafer substrate is placed on a spin coater for uniform distribution. The spin coater speed is 4000 r / min and the holding time is 1 min.

[0042] c. Place the silicon wafer substrate containing the solution from step b into the first high-temperature zone of the tube furnace, weigh 0.1g of sulfur powder into the corundum crucible, and then place the crucible in the second high-temperature zone upstream of the first high-temperature zone. The distance between the first high-temperature zone and the second high-temperature zone is 20cm.

[0043] d. Set the argon flow rate to 300 sccm and continuously introduce 99.999% high-purity argon into the tube furnace to remove other impurity gases inside the tube furnace and maintain the reaction under an argon atmosphere inside the tube for 15 minutes. After the reaction is completed, set the argon flow rate to 150 sccm and continuously introduce argon as the growth carrier gas.

[0044] e. Turn on the power switch of the flat plate electric field and adjust the voltage to keep the electric field strength of the flat plate constant at 200V / cm.

[0045] f. Heat the first high-temperature zone in step c at a rate of 20℃ / min until it reaches the reaction growth temperature of 850℃ and grows for 15 minutes; at the same time, heat the second high-temperature zone at a rate of 6℃ / min until it reaches the set temperature of 300℃ and grows for 3 minutes.

[0046] g. After the reaction growth is completed, the argon gas described in step d is continuously introduced until the temperature drops to room temperature. Then, the argon gas and the flat plate electric field power supply are turned off to obtain the product, a two-dimensional unidirectionally arranged transition metal chalcogenide single crystal MoS2.

[0047] Example 2:

[0048] The detailed steps of the method for preparing two-dimensional wafer-level MoS2 single crystals of the present invention are as follows:

[0049] a. Weigh 2.059 g of analytical grade sodium molybdate powder and place it in a 250 mL volumetric flask. Dilute to volume with deionized water to prepare a solution with a concentration of 0.04 mol / L.

[0050] b. The sodium molybdate solution obtained in step a is dropped onto a 1×1cm SiO2 / Si silicon wafer substrate that has undergone hydrophilic treatment, and the silicon wafer substrate is placed on a spin coater for processing. The spin coater rotates at 2000 r / min and is held for 2 min to ensure that the sodium molybdate solution is evenly distributed on the silicon wafer substrate.

[0051] c. Place the silicon wafer substrate treated by the spin coater in step b into the first high-temperature zone of the tube furnace, weigh 0.3g of sulfur powder into the corundum crucible, and then place the crucible in the second high-temperature zone upstream of the first high-temperature zone. The distance between the first high-temperature zone and the second high-temperature zone is 20cm.

[0052] d. Set the argon flow rate to 300 sccm and introduce 99.999% high-purity argon into the tube furnace to remove other impurity gases inside the tube furnace; maintain the reaction under an argon atmosphere inside the tube for 20 min; then, continuously introduce argon into the tube furnace at a flow rate of 250 sccm as the growth carrier gas.

[0053] e. Turn on the power switch of the flat plate electric field and adjust the voltage to maintain a constant electric field strength of 200V / cm.

[0054] f. Heat the first high-temperature zone in step c at a rate of 20℃ / min until it reaches the reaction growth temperature of 855℃ for growth; at the same time, heat the second high-temperature zone at a rate of 30℃ / min until it reaches the set temperature of 300℃, and set the growth time to 5min.

[0055] g. After the reaction growth is completed, the argon gas described in step d is continuously introduced until the temperature drops to room temperature. Then, the argon gas and the flat plate electric field power supply are turned off to obtain the product, two-dimensional single crystal MoS2.

[0056] Example 3:

[0057] The detailed steps of the method for preparing two-dimensional WS2 single crystal with a single growth orientation according to the present invention are as follows:

[0058] a. Weigh 2.938g of analytical grade sodium tungstate powder and place it in a 500mL volumetric flask. Dilute to volume with deionized water to prepare a solution with a concentration of 0.02mol / L.

[0059] b. The sodium tungstate solution obtained in step a is dropped onto a 1×1cm SiO2 / Si silicon wafer substrate that has undergone hydrophilic treatment, and the silicon wafer substrate is placed on a spin coater for processing. The spin coater rotates at 4000 r / min and is held for 1 min to ensure that the sodium tungstate solution is evenly distributed on the silicon wafer substrate.

[0060] c. Place the silicon wafer substrate treated by the spin coater in step b into the first high-temperature zone of the tube furnace, weigh 0.2g of sulfur powder into the corundum crucible, and then place the crucible in the second high-temperature zone upstream of the first high-temperature zone. The distance between the first high-temperature zone and the second high-temperature zone is 20cm.

[0061] d. Set the argon flow rate to 500 sccm and continuously introduce 99.999% high-purity argon into the tube furnace to remove other impurity gases inside the tube furnace. Maintain the reaction under an argon atmosphere inside the tube for 18 minutes. After the reaction is completed, continue to introduce argon into the tube furnace at a flow rate of 200 sccm as the growth carrier gas.

[0062] e. Turn on the power switch of the flat plate electric field and adjust the voltage to maintain a constant electric field strength of 200V / cm.

[0063] f. Heat the first high-temperature zone in step c at a rate of 20℃ / min until it reaches the reaction growth temperature of 850℃ for growth; at the same time, heat the second high-temperature zone at a rate of 30℃ / min until it reaches the set temperature of 300℃, and set the growth time to 5min.

[0064] g. After the reaction growth is completed, the argon gas described in step d is continuously introduced until the temperature drops to room temperature. Then, the argon gas and the flat plate electric field power supply are turned off to obtain the product, a two-dimensional single-oriented WS2 single crystal.

[0065] Example 4:

[0066] The detailed steps of the method for preparing two-dimensional wafer-level WS2 single crystals of the present invention are as follows:

[0067] a. Weigh 1.469 g of analytical grade sodium tungstate powder and place it in a 100 mL volumetric flask. Dilute to volume with deionized water to prepare a solution with a concentration of 0.05 mol / L.

[0068] b. The sodium tungstate solution obtained in step a is dropped onto a 1×1cm SiO2 / Si silicon wafer substrate that has undergone hydrophilic treatment, and the silicon wafer substrate is placed on a spin coater for processing. The spin coater rotates at 3000 r / min and is held for 1 min to ensure that the sodium tungstate solution is evenly distributed on the silicon wafer substrate.

[0069] c. Place the silicon wafer substrate treated by the spin coater in step b into the first high-temperature zone of the tube furnace, weigh 0.3g of sulfur powder into the corundum crucible, and then place the crucible in the second high-temperature zone upstream of the first high-temperature zone. The distance between the first high-temperature zone and the second high-temperature zone is 20cm.

[0070] d. Set the argon flow rate to 500 sccm and continuously introduce 99.999% high-purity argon into the tube furnace to remove other impurity gases inside the tube furnace. Maintain the reaction under an argon atmosphere inside the tube for 10 minutes. After the reaction is completed, continue to introduce argon into the tube furnace at a flow rate of 250 sccm as the growth carrier gas.

[0071] e. Turn on the power switch of the flat plate electric field and adjust the voltage to maintain a constant electric field strength of 300V / cm.

[0072] f. Heat the first high-temperature zone in step c at a rate of 20℃ / min until it reaches the reaction growth temperature of 860℃ for growth; at the same time, heat the second high-temperature zone at a rate of 30℃ / min until it reaches the set temperature of 280℃, and set the growth time to 5min.

[0073] g. After the reaction growth is completed, the argon gas described in step d is continuously introduced until the temperature drops to room temperature. Then, the argon gas and the flat plate electric field power supply are turned off to obtain the two-dimensional wafer-level WS2 single crystal.

[0074] Example 5:

[0075] A method for preparing two-dimensional MoS2 single crystals under no electric field conditions is basically the same as that in Example 1, except that:

[0076] In step e: the electric field strength is 0 V / cm.

[0077] Appendix Figure 9 This is an optical image of the discontinuous MoS2 grains prepared in Example 5 of the present invention. The prepared MoS2 domains are approximately 10 μm in size and have random growth orientations. In contrast, the two-dimensional transition metal chalcogenide domains prepared by the technical solution of the present invention have highly consistent growth orientations, enabling controllable preparation at the wafer-level single crystal level.

Claims

1. A method for preparing wafer-level single crystals by directional growth of two-dimensional transition metal chalcogenide single crystals under an electric field environment, characterized in that, The preparation method includes the following steps: a. Add metal oxophosphate powder to deionized water to prepare a solution with a concentration of 0.01–0.05 mol / L; by adjusting the concentration of the metal oxophosphate solution, small single crystals with the same crystal domain orientation are driven to splice together without grain boundaries to form wafer-level single crystals; The metal oxophosphate is any one of Na2MoO4, Na3VO4, Na2WO4, and NaNbO3; the particle size of the metal oxophosphate powder is ≤2μm; b. The metal oxophosphate solution obtained in step a is dropped onto the hydrophilically treated SiO2 / Si silicon wafer substrate, and the solution is evenly distributed on the silicon wafer substrate using a spin coater; c. Place the silicon wafer substrate coated with metal oxoate solution in step b into the first high-temperature zone of the tube furnace, and place sulfur powder or selenium powder into the second high-temperature zone upstream. The amount of sulfur powder added is 50-500 mg, and the amount of selenium powder added is 50-500 mg. d. Remove impurity gases from the atmosphere of the quartz tube in the tubular furnace by introducing 99.999% pure argon gas at a flow rate of 300-600 sccm to remove other gases in the quartz tube for 10-20 minutes; during the reaction, argon gas or an argon-hydrogen mixture is continuously introduced as the growth carrier gas. The flow rate of argon or argon-hydrogen mixture used as the growth carrier gas is 100-300 sccm, and the proportion of hydrogen in the argon-hydrogen mixture is 1-10%. e. Turn on the power switch of the flat plate electric field and adjust the voltage to maintain a constant electric field strength in the flat plate electric field; The electric field strength is 100–500 V / cm; f. The first high-temperature zone in step c is heated at a first heating rate to a reaction growth temperature of 750-900°C for growth, and the growth time is 3-10 min. At the same time, the second high-temperature zone is heated at a second heating rate to a set temperature of 150-350°C for a constant temperature time of 3-20 min. g. After the reaction growth is completed, argon or argon-hydrogen mixture as described in step d is continuously introduced until the temperature drops to room temperature. Then, the argon or argon-hydrogen mixture and the flat electric field power supply are turned off to obtain the product, a two-dimensional wafer-level transition metal chalcogenide single crystal.

2. The method for preparing wafer-level single crystals based on the directional growth of two-dimensional transition metal chalcogenide single crystals under an electric field environment according to claim 1, characterized in that: The spin coater used in step b has a rotation speed of 500–5000 r / min and a holding time of 30–120 s.

3. The method for preparing wafer-level single crystals based on the directional growth of two-dimensional transition metal chalcogenide single crystals under an electric field environment according to claim 1, characterized in that: In step c, the distance between the first high-temperature zone and the second high-temperature zone is 15-20 cm.

4. The method for preparing wafer-level single crystals based on the directional growth of two-dimensional transition metal chalcogenide single crystals under an electric field environment according to claim 1, characterized in that: In step f, the first heating rate is 10-20℃ / min, and the second heating rate is 5-40℃ / min.

Citation Information

Patent Citations

  • Method for growing single-crystal two-dimensional transitional metal sulphide