Molybdenum disulfide / titanium carbide MXene heterojunction catalyst and preparation method and application thereof
The synthetic molybdenum disulfide/titanium carbide MXene heterojunction catalyst was solved by wet chemical etching and electrostatic self-assembly technology, and the problems of unstable structure and insufficient catalytic activity of molybdenum disulfide electrocatalyst in the prior art were solved, and the acid-base Highly efficient electrocatalytic activity and stability in the environment.
Patent Information
- Application Number
- CN202310483486.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-04
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-04
AI Technical Summary
The existing molybdenum disulfide electrocatalysts have single steps in improving catalytic activity, no obvious effect, unstable structure, and difficult to show excellent electrocatalytic activity and stability in acid-base environments.
Thin layer of titanium-carbated MXene nanosheets were prepared by wet chemical etching, and the molybdenum disulfide/titanium-carbated MXene heterojunction catalyst was synthesized through functional group modification and electrostatic self-assembly methods to regulate its electronic structure and sulfur vacancy to form an efficient catalyst.
It significantly improves the catalytic activity and stability of the catalyst, and can show excellent electrocatalytic activity and efficient hydrogen adsorption performance in acid and alkali environment.
Smart Images

Figure CN116459852B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a molybdenum disulfide / titanium carbide MXene heterojunction electrocatalyst and a preparation method and application thereof, belonging to the field of new chemical material catalysis. Background Art
[0002] Compared with semiconductor phase MoS2, metal phase MoS2 exhibits higher conductivity and better catalytic activity. The inert basal plane of MoS2 can be activated by further introducing sulfur vacancies to increase defect states. These defect states are responsible for hydrogen adsorption, but excessive sulfur vacancy concentrations will produce higher surface energy, weaken the stability of the structure, and thus cause the performance to reach the upper limit, limiting the development of MoS2 electrocatalysts. Therefore, if efficient electrocatalysts are to be prepared, MoS2 must be regulated by scientific strategies to improve the active site density and poor conductivity. According to the inventors' research, in the past few years, the optimization methods used to improve the catalytic activity of MoS2 include phase change engineering, defect engineering, and in-situ growth to construct heterojunctions. However, these methods have relatively simple steps, unobvious improvement effects, unstable structures, etc., which are not conducive to practical applications. Summary of the invention
[0003] In view of the problems existing in the prior art, the present invention provides a preparation method and application of a molybdenum disulfide / titanium carbide MXene heterojunction catalyst. The present invention combines a variety of control methods to prepare a molybdenum disulfide / titanium carbide MXene heterojunction with controllable functional groups, and has the characteristics of high concentration of sulfur vacancies, effective regulation of electronic structure, effective charge transfer and greatly improved catalytic performance, and exhibits excellent electrocatalytic activity and stability in both acidic and alkaline environments.
[0004] The preparation method of the molybdenum disulfide / titanium carbide MXene heterojunction catalyst of the present invention comprises the following steps: wet chemically etching blocky titanium aluminum carbide to obtain thin-layer titanium carbide MXene nanosheets, performing functional group modification on the thin-layer titanium carbide MXene nanosheets to obtain functional group-modified titanium carbide MXene nanosheets; using a thin-layer molybdenum disulfide nanosheet dispersion as a precursor, doping with metal salts to obtain defective molybdenum disulfide nanosheets; and assembling thin-layer titanium carbide MXene nanosheets or functional group-modified titanium carbide MXene nanosheets and defective molybdenum disulfide nanosheets by an electrostatic self-assembly method to obtain the molybdenum disulfide / titanium carbide MXene heterojunction catalyst.
[0005] The LiF-HCl method is used to etch at 30-50°C for 24-48h to obtain a thin layer of titanium carbide MXene nanosheets with a size of 1-60 μm and a thickness of 1-50 nm; the thin layer of titanium carbide MXene nanosheets is functionally modified by ethylene glycol solvent thermal treatment, n-butyl lithium reduction or NaOH thermal treatment to obtain functional group-modified titanium carbide MXene nanosheets Ti3 C 2 -OH and Ti 3 C 2 -O.
[0006] The defective MoS2 nanosheet has a sheet size of <2 μm and a thickness of 0.67-3.0 nm, and phases include 2H phase, 1T phase and a mixed phase of 2H and 1T. The sulfur vacancy defect concentration of MoS2 is 5-35% of the Mo atoms, and the metal atom doping amount is 1-20% of the molar amount of MoS2. Specifically, bulk MoS2 (size <2 μm) is placed in an n-butyl lithium solution, treated at 10-30° C., a nitrogen atmosphere and an ultrasonic frequency of 80-100 Hz for 3-10 hours, washed with n-hexane, dried, and automatically peeled by adding deionized water. A thin layer of MoS2 nanosheet dispersion is obtained by centrifugal washing, and then a metal salt is added to the dispersion. After stirring and reacting in an inert atmosphere, the excess metal source is removed by water washing to obtain defective MoS2 nanosheets. After dispersion with deionized water, a dispersion with a concentration of 0.1-2 mg / mL is obtained.
[0007] The metal salt is one or more transition metal salts such as palladium salt, cobalt salt, zinc salt, copper salt and chromium salt.
[0008] The mass ratio of the electrostatically self-assembled thin-layer titanium carbide MXene nanosheets or functional group-modified titanium carbide MXene nanosheets to the defective molybdenum disulfide nanosheets is 1:0.05~0.5.
[0009] Another object of the present invention is to provide a molybdenum disulfide / titanium carbide MXene heterojunction catalyst prepared by the above method.
[0010] Another object of the present invention is to apply the molybdenum disulfide / titanium carbide MXene heterojunction catalyst in the electrolysis of water to produce hydrogen.
[0011] The beneficial effects of the present invention are as follows:
[0012] The method of the present invention combines the use of multiple controls to prepare a functional group-controllable molybdenum disulfide / titanium carbide MXene heterojunction catalyst. The heterojunction optimizes the local electronic structure of the interface between molybdenum disulfide and titanium carbide MXene, improves its adsorption energy for hydrogen, and enhances its catalytic activity and highly stable hydrogen evolution performance. The catalyst has the characteristics of high concentration of sulfur vacancies, effective regulation of electronic structure, effective charge transfer and greatly improved catalytic performance, and exhibits excellent electrocatalytic activity and stability in both acidic and alkaline environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is a SEM image of molybdenum disulfide nanosheets prepared in Example 1;
[0014] Figure 2This is a SEM image of the titanium carbide MXene nanosheet prepared in Example 1;
[0015] Figure 3 MoS2 / Ti 3 C 2 - F LSV curve of MXene heterojunction electrocatalyst for electrocatalytic hydrogen evolution in acidic medium;
[0016] Figure 4 MoS2 / Ti 3 C 2 - LSV curve of electrocatalytic hydrogen evolution of OH MXene heterojunction electrocatalyst in alkaline medium;
[0017] Figure 5 MoS2 / Ti 3 C 2 - LSV curves of electrocatalytic hydrogen evolution over O MXene heterojunction electrocatalyst in alkaline medium. DETAILED DESCRIPTION
[0018] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, and the protection scope of the present invention is not limited to the contents. The methods in the embodiments are conventional methods unless otherwise specified, and the reagents are conventional commercially available reagents or reagents prepared according to conventional methods unless otherwise specified. Example 1
[0019] 1. Take 1 g of molybdenum disulfide powder (size <2 μm) and 10 mL of n-butyl lithium solution (2.5 M, solvent is n-hexane, commercially available) in a Shrek tube under nitrogen atmosphere, maintain the ultrasonic frequency at 100 Hz and the temperature at 27 °C, wash with n-hexane after 5 h of intercalation, purge and dry with nitrogen, add deionized water to peel, and centrifuge and wash (sequentially centrifuge at 3000 rpm to retain sedimentation, disperse with water, centrifuge at 13000 rpm to retain sedimentation, disperse with water, centrifuge at 3000 rpm to retain suspension, and retain sedimentation at 13000 rpm, wash until pH is approximately equal to 8-9, and disperse with water) to obtain a dispersion of thin-layer molybdenum disulfide nanosheets. The SEM image of the thin-layer molybdenum disulfide nanosheets is shown in Figure 1 As can be seen from the figure, the original blocky MoS2 was peeled off into a few thin sheets; then 5.61 mg of palladium acetate powder was added to 40 mL of a 1 mg / mL thin-layer MoS2 nanosheet dispersion, stirred at room temperature for 12 h under a nitrogen atmosphere, and centrifuged and washed with water until pH = 7, to obtain defective MoS2 nanosheets with a sheet size of <2 μm, a thickness of 0.67-3 nm, a phase ratio of 1T and 2H phases of 3:1, and a defect concentration of 35%. After the defective MoS2 nanosheets were dispersed in water, a uniform dispersion of 1 mg / mL was obtained;
[0020] 2. In a 100 mL polytetrafluoroethylene container, add 3.12 g LiF to 40 mL 9 mol / L hydrochloric acid solution and mix well. Then, add 2 g titanium carbide Ti 3 AlC 2 Slowly add to the mixture, stir in a constant temperature oil bath at 50 ° C for 24 hours, and then centrifuge and wash the reactants at 10000 rpm for 6 times (5 minutes each time) until the supernatant is neutral. The deposit obtained by the last centrifugal washing is dispersed with deionized water, and then ultrasonically treated at room temperature for 1 hour, centrifuged at 3000 rpm for 1 hour to remove the product with poor stripping effect, collect the dark green stable supernatant, and dilute with deionized water to obtain a thin layer of Ti with a concentration of 8 mg / mL. 3 C 2 -F MXene nanosheet dispersion, nanosheet size 10 μm, thickness 2 nm; SEM image of nanosheets is shown in Figure 2 From the figure, it can be seen that the blocky titanium carbide is peeled off into transparent thin sheets; take 19mL Ti 3 C 2 The dispersion of -F MXene nanosheets was diluted with 80 mL of deionized water, and then 1 mL of polydimethyl ammonium chloride was added dropwise. After stirring at room temperature for 4 h, it was centrifuged and washed three times at 10000 rpm (5 min each time). The washed precipitate was ultrasonically dispersed with deionized water for 1 h to obtain a positively charged Ti with a concentration of 8 mg / mL. 3 C 2 -F MXene nanosheet dispersion;
[0021] 3. Press Ti 3 C 2 The mass ratio of -F MXene nanosheets to defective MoS2 nanosheets is 1:0.06, which converts the positively charged Ti 3 C 2 -F MXene nanosheet dispersion was added dropwise to the defective MoS2 nanosheet dispersion in step 1, and stirring was continued for 30 min after the addition was completed to obtain MoS2 / Ti 3 C 2 -F MXene heterojunction catalyst;
[0022] 4. Using a water electrolysis device containing an anode and a cathode, the catalyst prepared in this embodiment was applied to the electrolysis of water for hydrogen evolution reaction. The alkaline hydrogen evolution test was carried out with an electrolyte of 1M KOH and a voltage range of 0.2 to -1.2V. The results are shown in FIG. Figure 3 , defective MoS2 / Ti 3 C 2 -F MXene heterojunction electrocatalysts exhibit excellent hydrogen evolution performance under alkaline conditions. Example 2
[0023] 1. Take 1 g of molybdenum disulfide powder (size <2 μm) and 10 mL of n-butyl lithium solution (2.5 M, solvent is n-hexane, commercially available), react in a Shrek tube in a nitrogen atmosphere, maintain the ultrasonic frequency at 90 Hz, the temperature at 25 ° C, wash with n-hexane after intercalation for 4 hours, purge with nitrogen to dry, add deionized water to peel, centrifuge and wash (same as Example 1) to obtain a thin layer of molybdenum disulfide nanosheet dispersion, then add 2.8 mg of palladium acetate powder to 40 mL of the dispersion with a concentration of 1 mg / mL, stir at room temperature for 12 hours under a nitrogen atmosphere, and centrifuge and wash with water until pH = 7 to obtain a defective molybdenum disulfide nanosheet with a sheet size of <2 μm, a thickness of 0.67-3 nm, a phase ratio of 1T and 2H phases of 3:1, and a defect concentration of 22%. After the defective molybdenum disulfide nanosheet is dispersed in water, a uniform dispersion of 1 mg / mL is obtained;
[0024] 2. Prepare dark green supernatant Ti by referring to step 2 of Example 1 3 C 2 -F MXene nanosheets, after freeze drying, 15 mL of ethylene glycol was added to 0.5 g of the freeze-dried sample, and after stirring for 30 min, the suspension was transferred to a 20 mL stainless steel autoclave with a polytetrafluoroethylene substrate and subjected to solvent thermal treatment at 160 °C for 24 h. The product was then centrifuged and washed three times with deionized water (3000 rpm / 5 min), and the washed precipitate was ultrasonically dispersed with deionized water to obtain a TiO2 solution with a concentration of 8 mg / mL. 3 C 2 -OHMXene uniform dispersion; take 19mL Ti 3 C 2 The -OH MXene nanosheet dispersion was diluted with 80 mL of deionized water, and then 1 mL of polydiallyl dimethyl ammonium chloride was added dropwise. After stirring at room temperature for 4 h, it was centrifuged and washed three times at 10000 rpm (5 min each time). The washed precipitate was ultrasonically dispersed with deionized water for 1 h to obtain a positively charged Ti-OH nanosheet dispersion with a concentration of 8 mg / mL. 3 C 2 -OHMXene nanosheet dispersion;
[0025] 3. Press Ti 3 C 2 The mass ratio of the defective MoS2 nanosheets to the -OH MXene nanosheets is 1:0.06, which converts the positively charged Ti 3 C 2 -OH MXene nanosheet dispersion was added dropwise to the defective MoS2 nanosheet dispersion in step 1, and stirring was continued for 30 min after the addition was completed to obtain MoS2 / Ti 3 C2 -OH MXene heterojunction catalyst;
[0026] 4. Using a water electrolysis device containing an anode and a cathode, the catalyst prepared in this embodiment was applied to the hydrogen evolution reaction by water electrolysis, with the electrolyte being 0.5 M H 2 SO 4 , the acidic hydrogen evolution test was carried out in the voltage range of 0.2 ~ -1.2V, and the results are shown in Figure 4 , defective MoS2 / Ti 3 C 2 -OH MXene heterojunction electrocatalysts exhibit excellent hydrogen evolution performance under acidic conditions. Example 3
[0027] 1. Take 1 g of molybdenum disulfide powder (size <2 μm) and 10 mL of n-butyl lithium solution (2.5 M, solvent is n-hexane, commercially available), react in a Shrek tube in a nitrogen atmosphere, maintain the ultrasonic frequency at 100 Hz, the temperature at 20°C, wash with n-hexane after intercalation for 5 hours, purge with nitrogen to dry, add deionized water to peel, centrifuge and wash (same as Example 1) to obtain a thin layer of molybdenum disulfide nanosheet dispersion, then add 1.4 mg of palladium acetate powder to 40 mL of the dispersion with a concentration of 1 mg / mL, stir at room temperature for 12 hours under a nitrogen atmosphere, and centrifuge and wash with water until pH=7 to obtain a defective molybdenum disulfide nanosheet with a sheet size of <2 μm, a thickness of 0.67-3 nm, a phase ratio of 1T and 2H phases of 3:1, and a defect concentration of 13%. The defective molybdenum disulfide nanosheet is dispersed in water to obtain a 1 mg / mL uniform dispersion;
[0028] 2. Prepare dark green supernatant Ti by referring to step 2 of Example 1 3 C 2 -F MXene nanosheets, freeze-dried, 1 g of the freeze-dried sample and 20 mL of n-butyl lithium solution (2.5 M, the solvent is n-hexane, commercially available) were taken, and the temperature was maintained at 50 °C in a Shrek tube under a nitrogen atmosphere for 10 days, and then washed four times with n-hexane, and then added with deionized water for dispersion and deposition. After ultrasonic treatment for 2 h, the washed precipitate was centrifuged at 10000 rpm and washed several times with water. The washed precipitate was ultrasonically dispersed with deionized water to obtain a Ti with a concentration of 8 mg / mL 3 C 2 -O dispersion; take 19mL Ti 3 C 2 The dispersion of -O MXene nanosheets was diluted by adding 80 ml of deionized water, and then 1 mL of polydimethyl ammonium chloride was added dropwise. After stirring at room temperature for 4 h, it was centrifuged and washed three times at 10000 rpm (5 min each time). The washed precipitate was ultrasonically dispersed with deionized water for 1 h to obtain a positively charged TiO nanosheet dispersion with a concentration of 8 mg / mL.3 C 2 -O MXene nanosheet dispersion;
[0029] 3. Press Ti 3 C 2 The mass ratio of the defective MoS2 nanosheets to the defective MoS2 nanosheets is 1:0.06, which converts the positively charged Ti 3 C 2 -O MXene nanosheet dispersion was added dropwise to the defective MoS2 nanosheet dispersion in step 1, and stirring was continued for 30 min after the addition was completed to obtain defective MoS2 / Ti 3 C 2 -O MXene heterojunction catalyst;
[0030] 4. Using a water electrolysis device containing an anode and a cathode, the catalyst prepared in this embodiment was applied to the hydrogen evolution reaction by water electrolysis, with the electrolyte being 0.5 M H 2 SO 4 , the acidic hydrogen evolution test was carried out in the voltage range of 0.2 ~ -1.2V, and the results are shown in Figure 5 , defective MoS2 / Ti 3 C 2 -O MXene heterojunction electrocatalysts exhibit excellent hydrogen evolution performance under acidic conditions.
Claims
1. A method for preparing a molybdenum disulfide / titanium carbide MXene heterojunction catalyst, characterized in that: Blocky titanium aluminum carbide is etched by wet chemical method to obtain thin titanium carbide MXene nanosheets, and the thin titanium carbide MXene nanosheets are functionally modified to obtain functional group-modified titanium carbide MXene nanosheets; a thin layer of molybdenum disulfide nanosheet dispersion is used as a precursor, and metal salts are doped to obtain defective molybdenum disulfide nanosheets; Take 19 mL of thin-layer titanium carbide MXene nanosheets or functional group-modified titanium carbide MXene nanosheet dispersion, add 80 mL of deionized water for dilution, then drop 1 mL of polydiallyl dimethyl ammonium chloride, stir at room temperature for 4 hours, centrifuge and wash three times at 10000 rpm, each time for 5 minutes, and ultrasonically disperse the washed precipitate with deionized water for 1 hour to obtain a positively charged thin-layer titanium carbide MXene nanosheet or positively charged functional group-modified titanium carbide MXene nanosheet dispersion with a concentration of 8 mg / mL; The MoS2 / Titanium Carbide MXene heterojunction catalyst is obtained by assembling positively charged thin-layer titanium carbide MXene nanosheets or positively charged functional group-modified titanium carbide MXene nanosheets and defective MoS2 nanosheets using an electrostatic self-assembly method. The wet chemical etching of bulk titanium carbide aluminum is carried out by using the LiF-HCl method at 30-50°C for 24-48h, and the obtained thin-layer titanium carbide MXene nanosheets have a size of 1-60 μm and a thickness of 1-50 nm. The defective MoS2 nanosheets have a sheet size of <2 μm and a thickness of 0.67-3.0 nm. The phases include 2H phase, 1T phase and a mixed phase of 2H and 1T. The sulfur vacancy defect concentration of MoS2 is 5-35% of the Mo atoms, and the metal atom doping amount is 1-20% of the molar amount of MoS2. Specifically, the bulk MoS2 with a size of <2 μm is placed in an n-butyl lithium solution, treated at 10-30°C, a nitrogen atmosphere and an ultrasonic frequency of 80-100 Hz for 3-10 hours, washed with n-hexane, dried, and automatically peeled by adding deionized water. The thin layer MoS2 nanosheet dispersion is obtained by centrifugal washing, and then a metal salt is added to the dispersion. After stirring and reacting in an inert atmosphere, the excess metal source is removed by water washing to obtain the defective MoS2 nanosheets. The metal salt is a palladium salt; The functional group-modified titanium carbide MXene nanosheets are Ti3C2-OH MXene nanosheets and Ti3C2-O MXene nanosheets, and the thin-layer titanium carbide MXene nanosheets are thin-layer Ti3C2-F MXene nanosheets.
2. The method for preparing the molybdenum disulfide / titanium carbide MXene heterojunction catalyst according to claim 1, characterized in that: The functional group modification method is ethylene glycol solvent thermal treatment method, n-butyl lithium reduction method or NaOH thermal treatment method.
3. The method for preparing the molybdenum disulfide / titanium carbide MXene heterojunction catalyst according to claim 1, characterized in that: The mass ratio of electrostatically self-assembled positively charged thin-layer titanium carbide MXene nanosheets or positively charged functional group-modified titanium carbide MXene nanosheets to defective molybdenum disulfide nanosheets is 1:0.05~0.
5.
4. A molybdenum disulfide / titanium carbide MXene heterojunction catalyst prepared by the preparation method of the molybdenum disulfide / titanium carbide MXene heterojunction catalyst according to any one of claims 1 to 3.
5. Application of the molybdenum disulfide / titanium carbide MXene heterojunction catalyst according to claim 4 in hydrogen production by water electrolysis.
Citation Information
Patent Citations
Preparation method and application of metal-doped 2H-phase molybdenum disulfide electrocatalyst
CN115029724A