Aqueous inkjet inks for non-absorbent printing substrates
By using a water-based composition of low concentration calcium salt and low acid value polyurethane binder in water-based inkjet ink, the problem of adhesion and fixation performance of water-based inkjet ink on low-absorbent printing substrates is solved, and high performance is achieved. Quality printed images and long-term storage stability.
Patent Information
- Application Number
- CN202211549250.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-05
AI Technical Summary
Existing water-based inkjet inks have poor adhesion to low-absorbent printing substrates, poor ink fixation properties after drying, and are prone to spreading or bleeding, resulting in unsatisfactory printed images and durability issues, and are unstable when stored at high temperatures.
A water-based composition using low concentration calcium salt as fixative, low acid value polyurethane binder and low acid value dispersant is applied to the printing substrate through an inkjet print head to form a high viscosity of less than 30 mPa·s The ink film ensures the stability and overprinting performance of the ink.
Achieving high image quality printed images on non-absorbent printing substrates, resisting scratches and blurring, and maintaining long-term storage stability at high temperatures.
Abstract
Description
Technical Field
[0001] The present invention relates to an aqueous inkjet ink and a printing method, in which the aqueous inkjet ink is used. Background Art
[0002] Inkjet printing methods are known in the printing industry, in which one or more inkjet print heads output inkjet inks in a controllable manner via a large number of inkjet nozzles onto a printing substrate. After a drying process in the printer, a finished printed image is obtained. In principle, UV inkjet inks and aqueous inkjet inks can be used in the inkjet printing method, wherein UV inkjet inks are usually dried by the action of ultraviolet radiation, and aqueous inkjet inks are dried by heating, usually by irradiation with infrared radiation.
[0003] It is known that certain printing substrates do not have satisfactory performance when printed with aqueous inkjet inks. This is particularly true for those printing substrates that have a low absorption capacity for such inkjet inks. For example, printing directly on polyethylene plastic films can result in the printed image being prone to stains and smears. Therefore, in order to avoid such undesirable results, it is known that a primer is applied to the printing substrate before the actual inkjet printing. This primer makes it possible to print a perfect printed image with conventional aqueous inkjet inks in a subsequent step.
[0004] Typically, printing is not done in single colors, but in multiple colors, for example in the CMYK color space. The problem here is that the aqueous inkjet inks used do not have satisfactory ink fixation properties after drying. This means that if the dried aqueous inkjet ink is overprinted by another aqueous inkjet ink, the last applied ink may spread or bleed (in English, bleed) and thus lead to unsatisfactory printed images. Moreover, the commercial requirements for the durability of the printed image may also be compromised.
[0005] US 2017 / 0321084 A1 describes an aqueous primer for smooth paper substrates, which enables better printed images and better durability during inkjet printing. The aqueous primer comprises a pigment, a multivalent salt and a polyurethane dispersion as a binder. There is no description of applying the primer by means of inkjet printing.
[0006] EP 2 718 110 A1 describes a white pretreatment composition for inkjet printing comprising a binder, a polyvalent metal salt, a latex resin and titanium dioxide particles.
[0007] EP 3 798 276 A1 describes an aqueous lacquer composition for producing lacquer layers by the inkjet process, wherein the aqueous lacquer composition comprises a binder and a polyurethane.
[0008] WO 2020 / 046341 A1 describes a primer for inkjet printing, which comprises a polyvalent metal salt, a cationic polymer and water. Also described is an inkjet ink comprising a pigment, a polyurethane-based binder and water.
[0009] WO 2007 / 035505 A1 describes aqueous inkjet inks comprising titanium dioxide and a polyurethane binder. The aqueous inkjet inks should be particularly suitable for printing textiles.
[0010] Primers and inkjet inks described in the prior art have disadvantages. On the one hand, they cannot be applied to the printing substrate by means of inkjet printing in part. On the other hand, the described primers and inkjet inks are partially unsuitable for printing printing substrates with low absorption capacity. In addition, the described primers and inkjet inks cannot be overprinted with other aqueous inkjet inks in a dry state without causing defective printed images. Here, the ink of subsequent printing may fade (bleed), and may produce a non-scratch-resistant printing result. Partly, the compositions described in the prior art are unstable in storage over a long period of time, particularly at elevated temperatures, such as in inkjet printers.
[0011] There is still a need for aqueous inkjet inks that avoid the above-mentioned disadvantages. These aqueous inkjet inks should be advantageously applied to non-absorbent printing substrates by inkjet printing and allow satisfactory overprinting with other aqueous inkjet inks. Aqueous inkjet inks should also be storage-stable and not lose their advantageous properties even when stored for a long time at high temperatures. Summary of the invention
[0012] The applicant has now surprisingly found that water-based compositions comprising low concentrations of calcium salts as fixing agents, low acid polyurethane binders, low acid dispersants and pigments are compatible with conventional inkjet print heads and can be printed by means of inkjet printing, wherein a well-adhering ink film is obtained on a weakly water-absorbing printing substrate, which ink film can be advantageously overprinted. As a result, a printed image of high image quality is obtained, which is resistant to scratching or blurring. These compositions are storage-stable even when exposed to high temperatures for a longer period of time.
[0013] Therefore, a first aspect of the present invention relates to an inkjet ink comprising the following components:
[0014] a) at least one pigment;
[0015] b) at least one dispersant having an acid value of less than 20 mg KOH / g relative to the total dispersant b);
[0016] c) at least one fixing agent selected from multivalent calcium salts, wherein the amount of the at least one fixing agent is in the range of 0.05 to 5% by weight relative to the total inkjet ink;
[0017] d) at least one binder selected from polyurethanes having an acid value of less than 20 mgKOH / g relative to the total binder d);
[0018] e) water;
[0019] The viscosity of the inkjet ink is less than 30 mPa·s (measured by a cone-plate viscometer at 25° C.).
[0020] In a preferred embodiment, the inkjet ink of the present invention has a viscosity of less than 20 mPa·s (measured by cone and plate viscometer at 25° C.), particularly preferably less than 10 mPa·s (measured by cone and plate viscometer at 25° C.).
[0021] According to the invention, polyurethane is used as binder d). Binder d) is required to achieve sufficient adhesion of the inkjet ink of the invention to non-absorbent printing substrates.
[0022] The acid value of the at least one binder d) is less than 20 mg KOH / g relative to the total binder d). In a preferred embodiment, the acid value of the at least one binder d) is less than 10 mg KOH / g relative to the total binder d). The acid value indicates the mass of potassium hydroxide required to neutralize one gram of the corresponding dispersant or binder in milligrams. The determination of the acid value is described, for example, in DIN ISO 2114.
[0023] In a preferred embodiment, the at least one binder d) is selected from nonionic and anionic polyurethanes, preferably nonionic and weakly anionic polyurethanes. The distinction between nonionic and anionic or weakly anionic polyurethanes is familiar in principle to those skilled in the art. Polyurethanes that do not contain ionic groups are nonionic polyurethanes. If the polymer backbone of the polyurethane has side chains with anionic groups such as carboxyl or sulfonic acid groups, then as long as the polymer does not contain or contains only a small amount of cationic groups, it is usually anionic polyurethane. The side chains may also include cationic groups, such as amino groups, which may at least partially neutralize the anionic groups. The degree of the anionic nature of the polymer may be described by the acid value.
[0024] Polyurethanes are known in principle to the person skilled in the art and are obtained by polycondensation of one or more polyisocyanates, usually diisocyanates, and one or more polyols, usually diols. Examples of polyisocyanates are aromatic, araliphatic, aliphatic or cycloaliphatic diisocyanates, for example xylene diisocyanate, tetramethylene diisocyanate, 1,12-diisocyanatododecane, hexamethylene diisocyanate, 2,3,3-trimethylhexamethylene diisocyanate, 1,4-cyclohexene diisocyanate, 4,4'-cyclohexylmethane diisocyanate, 4,4'-cyclohexylmethane diisocyanate, 1,4-phenylene diisocyanate, 2,6-toluene diisocyanate, 2,4-toluene diisocyanate, 1,5-naphthalene diisocyanate, 2,4'-diphenyldimethylmethane isocyanate, 4,4'-diphenylmethane isocyanate or 4,4'-dimethylmethane isocyanate. Examples of polyols are alkane diols, such as ethylene glycol, polyethylene glycol, propylene glycol, tetramethylene glycol, polytetramethylene glycol, 1,6-hexanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, 3-methyl-1,5-pentanediol, 1,9-nonanediol or 2-methyl-1,8-octanediol.
[0025] The polyurethane of the present invention can be used as homopolymer or copolymer, preferably copolymer with polyester, polyether or polycarbonate. These preferred copolymers are polyurethanes whose polyurethane units and polyester units or polyether units or polycarbonate units are present together in the polymer chain, or in blocks as block polymers, or disordered. The linking of polyurethane units and polyester units can be carried out, for example, through the free hydroxyl groups of the polyol component of the polyurethane or polyester, which can react with isocyanate groups or carboxyl groups.
[0026] Polyesters are known in principle to those skilled in the art and can be obtained by polycondensation of polyols such as the above-mentioned alkanols with divalent or polyvalent carboxylic acids. Examples of divalent or polyvalent carboxylic acids are phthalic acid, isophthalic acid, terephthalic acid, maleic acid, fumaric acid, adipic acid and sebacic acid.
[0027] Polyethers are known in principle to the person skilled in the art and are, for example, polyether polyols comprising ethyleneoxy units or propyleneoxy units.
[0028] Polycarbonates are also known in principle to the person skilled in the art. These may be polycarbonate polyols obtained, for example, by reacting diols such as 1,2-propylene glycol, 1,4-butanediol or 1,6-hexanediol with diaryl carbonates such as diphenyl carbonate or phosgene.
[0029] According to the invention, preference is given to using polyurethane homopolymers, polyester polyurethanes, polycarbonate polyurethanes and mixtures thereof, particularly preferably polyester polyurethanes, polycarbonate polyurethanes and mixtures thereof as binders d).
[0030] The amount of the at least one binder d) is preferably 1 to 20% by weight (relative to the total inkjet ink), particularly preferably in the range of 3-15% by weight (relative to the total inkjet ink), particularly preferably in the range of 4 to 10% by weight (relative to the total inkjet ink).
[0031] The inkjet ink of the present invention comprises at least one fixing agent c) selected from polyvalent calcium salts. Calcium chloride, calcium acetate, calcium nitrate and mixtures thereof are preferred, and calcium chloride is particularly preferred as fixing agent c).
[0032] The inkjet ink of the present invention comprises the at least one fixing agent c) in an amount in the range of 0.05-5% by weight (relative to the total inkjet ink), preferably in the range of 0.1-4% by weight (relative to the total inkjet ink), and particularly preferably in the range of 0.5 to 3% by weight (relative to the total inkjet ink).
[0033] The inkjet ink of the present invention comprises at least one dispersant b). The dispersant b) is required to ensure sufficient stabilization of the pigment a) in the inkjet ink. The dispersant b) generally comprises a surfactant-like structure with pigment affine groups, which attaches to the pigment particles and protects them from agglomeration. In a preferred embodiment, the at least one dispersant b) is selected from nonionic and anionic dispersants, preferably nonionic and weakly anionic dispersants. Suitable dispersants are not only electrostatically stable, i.e. ionic dispersants, but also sterically stable, i.e. nonionic dispersants. The at least one dispersant b) can be, for example, a polymer comprising acrylic acid or methacrylic acid units.
[0034] The at least one dispersant b) has an acid value of less than 20 mg KOH / g relative to the total dispersant b). In a preferred embodiment, the at least one dispersant b) has an acid value of less than 10 mg KOH / g relative to the total dispersant b). The determination of the acid value can be carried out as expressed above for the binder d).
[0035] The amount of the at least one dispersant b) is preferably in the range of 0.1 to 10% by weight (relative to the total inkjet ink), particularly preferably in the range of 1 to 8% by weight (relative to the total inkjet ink).
[0036] The inkjet ink of the present invention comprises at least one pigment a). The at least one pigment a) is used as a colorant and is preferably selected from white pigments. This makes it particularly advantageous to print a white primer on a printed substrate, which can advantageously be overprinted with a colored aqueous inkjet ink.
[0037] The at least one pigment a) is preferably selected from inorganic oxides. In a particularly preferred embodiment, it is titanium dioxide. The at least one pigment a) is preferably used in the form of nanoparticles or microparticles. The at least one pigment a) can also be surface-functionalized, for example with aluminum or an inorganic aluminum compound such as aluminum oxide.
[0038] The inkjet ink of the present invention comprises the at least one pigment a) in an amount ranging from 1 to 30% by weight (relative to the total inkjet ink), particularly preferably in an amount ranging from 2 to 20% by weight (relative to the total inkjet ink).
[0039] The inkjet ink of the present invention comprises water e). The amount of water e) in the inkjet ink of the present invention is preferably at least 20% by weight (relative to the total inkjet ink), particularly preferably at least 40% by weight (relative to the total inkjet ink), and more particularly preferably at least 50% (relative to the total inkjet ink). In a preferred embodiment, the amount of water e) is in the range of 20 to 95% by weight (relative to the total inkjet ink), particularly preferably in the range of 50 to 80% by weight (relative to the total inkjet ink).
[0040] The inkjet ink of the present invention may include other components known in principle for aqueous inkjet inks, such as humectants (such as ethylene glycol or 1,3-butanediol), wetting agents (such as compounds with siloxane groups in particular), defoamers, buffers, biocides, etc.
[0041] The object of the present invention also includes a printing method using the inkjet ink of the present invention. Therefore, another aspect of the present invention relates to a printing method comprising the following steps:
[0042] i) providing a printing substrate;
[0043] ii) inkjet printing at least one inkjet ink according to the present invention onto a printing substrate;
[0044] iii) drying the inkjet ink printed in step (ii);
[0045] iv) inkjet printing at least one additional inkjet ink on the inkjet ink dried in step iii);
[0046] v) Drying the further inkjet ink printed in step iv).
[0047] As the inkjet ink of the present invention in step ii), preferably the preferred inkjet ink of the present invention described above is suitable.
[0048] As further inkjet ink in step iv), water-based inkjet inks are preferred, in particular inkjet inks having a water content of at least 20% by weight (relative to the total inkjet ink), which dry substantially by evaporation of said water.
[0049] In a preferred embodiment, the drying in steps iii) and v) is respectively carried out by heating, for example by IR radiation of an infrared dryer in an inkjet printer. During the drying process of the aqueous inkjet ink, the water contained in the ink is substantially completely removed, thereby obtaining a dried inkjet ink.
[0050] In a further preferred embodiment, the water absorption capacity of the printed substrate is less than 10 g of water / kg of printed substrate, particularly preferably less than 5 g of water / kg of printed substrate and particularly preferably less than 1 g of water / kg of printed substrate.
[0051] As printing substrate, preferred are plastics such as polyethylene, polypropylene or polyethylene terephthalate, which can be printed in an inkjet printer in particular as a film web or in the form of a label. In addition, as printing substrate, also preferred are printing substrates having at least one surface with a low water absorption capacity of less than 10 g water / kg surface material, preferably less than 5 g water / kg surface material and particularly preferably less than 1 g water / kg surface material. It can preferably be, for example, a plastic surface, a metal surface or a combination thereof. In a particularly preferred embodiment, the printing substrate is a paper or cardboard coated with plastic and / or metal, for example with a plastic foil and / or a metal foil.
[0052] The inkjet inks of the invention are characterized by simple printability in commercial inkjet printers, high storage stability, adhesion to non-water-absorbing surfaces with high scratch resistance and particularly favorable overprintability with other water-based inkjet inks.
[0053] Example
[0054] raw material
[0055] Pigment 1: 2066(≥95%Titanium dioxide)
[0056] Pigment 2: Titanium Dioxide RDIS (95% titanium dioxide)
[0057] Dispersant 1: 3800(polymer, slightly anionic dispersant)
[0058] Dispersant 2: DISPERBYK-190 (aqueous solution of a high molecular block copolymer with pigment affine groups, acid value 10 mg KOH / g)
[0059] Dispersant 3: DISPERBYK-2010 (aqueous emulsion of a structured acrylate copolymer with pigment affine groups)
[0060] Fixative 1: Calcium chloride
[0061] Binder 1: PrintRite DP 380
[0062] Binder 2: PrintRite DP 375 (aqueous polyurethane dispersion with a solids content of 30 to 34% and a pH of 4 to 8)
[0063] Binder 3: XW-UM3
[0064] Binder 4: R-9340 (aqueous nonionic polyester polyurethane dispersion, solid content 40%, pH 6.8)
[0065] Binder 5: D-2301
[0066] Binder 6: Takelac W-6355 (waterborne polycarbonate polyurethane dispersion)
[0067] Binder 7: PN 60 (modified polyethyleneimine) (comparison)
[0068] Binder 8: Antara 430 (styrene-vinyl pyrrolidone copolymer) (comparison)
[0069] Binder 9: VA73W (vinyl pyrrolidone-vinyl alcohol copolymer) (comparison)
[0070] Wetting agent 1: Twin 4000 (Silicone-based wetting agent)
[0071] Wetting agent 2: Twin 4100 (Silicone-based wetting agent)
[0072] Wetting agent 3: Twin 4200 (Silicone-based wetting agent)
[0073] Wetting agent 4: Wet 280 (Silicone-based wetting agent)
[0074] Wetting agent 5: TRITON HW-1000 (non-ionic wetting agent)
[0075] Defoamer 1: AD01
[0076] Humectant 1: Ethylene glycol
[0077] Humectant 2: 1,3-Butanediol
[0078] General approach
[0079] Pigment, dispersant, defoamer and water are mixed separately with a high shear mixer. The mixing is continued until the particle size is no longer reduced. Then the fixative, binder, wetting agent and moisturizer are added and mixed again with the high shear mixer until a uniform mixture is obtained.
[0080] The viscosity is measured according to DIN ISO 3219 by means of a cone and plate viscometer at 25°C.
[0081] The redispersibility of the sediment was measured by rolling the sample container at room temperature for 5 min.
[0082] Particle size measurement by dynamic light scattering
[0083] Storage stability measurement
[0084] The redispersibility of the deposits was measured after a test period of 28 days at 60° C. in a temperature-controlled cabinet. Only complete redispersibility was acceptable.
[0085] After 28 days of testing at 60°C in a temperature controlled cabinet, the changes in viscosity, pH and particle size were also determined using the above measurement methods. A viscosity change of no more than ±1 mPa·s is acceptable. A pH change of no more than -1 is acceptable. A particle size change of no more than ±80 nm is acceptable.
[0086] Example 1
[0087] 15% by weight Pigment 1
[0088] 1,5% by weight Dispersant 1
[0089] 1% by weight Fixative 1
[0090] 5% weight percentage binder 1
[0091] 1% by weight wetting agent 1
[0092] 0.25% by weight defoamer 1
[0093] 10% by weight Moisturizer 1
[0094] 66.25% by weight water
[0095] Viscosity: 3.1 mPa·s pH: 8.1
[0096] Change in viscosity after the test period: +0.4 mPa·s Change in pH after the test period: -0.1 Redispersibility of sediment after the test period: Yes Change in particle size after the test period: Acceptable Example 2
[0097] 15% by weight Pigment 1
[0098] 1.5% by weight Dispersant 1
[0099] 1% by weight Fixative 1
[0100] 5% weight percentage binder 1
[0101] 1% by weight wetting agent 2
[0102] 0.25% by weight defoamer 1
[0103] 10% by weight Moisturizer 1
[0104] 66.25% by weight Water Viscosity: 2.7 mPa·s pH: 8.2
[0105] Change in viscosity after the test period: +0.4 mPa·s Change in pH after the test period: -0.1 Redispersibility of sediment after the test period: Yes Change in particle size after the test period: Acceptable Example 3
[0106] 15% by weight Pigment 1
[0107] 1.5% by weight Dispersant 1
[0108] 1% by weight Fixative 1
[0109] 5% weight percentage binder 1
[0110] 1% by weight wetting agent 3
[0111] 0.25% by weight defoamer 1
[0112] 10% by weight Moisturizer 1
[0113] 66.25% by weight Water Viscosity: 2.9 mPa·s pH: 8.1
[0114] Change in viscosity after the test period: 0 mPa·s Change in pH after the test period: 0 Redispersibility of sediment after the test period: Yes Change in particle size after the test period: Acceptable Example 4
[0115] 15% by weight Pigment 1
[0116] 1.5% by weight Dispersant 1
[0117] 1% by weight Fixative 1
[0118] 5% weight percentage binder 1
[0119] 1% by weight wetting agent 4
[0120] 0.25% by weight defoamer 1
[0121] 10% by weight Moisturizer 1
[0122] 66.25% by weight Water Viscosity: 2.9 mPa·s pH: 8.3
[0123] Change in viscosity after the test period: +0.2 mPa·s Change in pH after the test period: -0.1 Redispersibility of sediment after the test period: Yes Change in particle size after the test period: Acceptable Example 5
[0124] 15% by weight Pigment 2
[0125] 1.5% by weight Dispersant 1
[0126] 1% by weight Fixative 1
[0127] 5% weight percentage binder 4
[0128] 0.25% by weight defoamer 1
[0129] 10% by weight Moisturizer 2
[0130] 67.25% by weight Water Viscosity: Undetermined
[0131] pH: 8.5
[0132] Change in viscosity after the test period: Not determined Change in pH after the test period: -0.8 Redispersibility of sediment after the test period: Yes Change in particle size after the test period: Acceptable Example 6
[0133] 15% by weight Pigment 2
[0134] 1.5% by weight Dispersant 3
[0135] 1% by weight Fixative 1
[0136] 5% by weight binder 2
[0137] 0.25% by weight defoamer 1
[0138] 5% by weight Moisturizer 1
[0139] 72.25% by weight Water Viscosity: 4.5 mPa·s pH: 8.1
[0140] Change in viscosity after the test period: 0 mPa·s Change in pH after the test period: -1 Redispersibility of sediment after the test period: Yes Change in particle size after the test period: Acceptable Example 7
[0141] 15% by weight Pigment 1
[0142] 1.5% by weight Dispersant 2
[0143] 1% by weight Fixative 1
[0144] 5% weight percentage binder 5
[0145] 0.25% by weight defoamer 1
[0146] 5% by weight Moisturizer 1
[0147] 72.25% by weight Water Viscosity: 3.5 mPa·s pH: 8.7
[0148] Viscosity change after test period: 0 mPa·s pH change after test period: -0.6 Sediment redispersibility after test period: Yes Particle size change after test period: Acceptable Example 8
[0149] 15% by weight Pigment 1
[0150] 1.2% by weight Dispersant 1
[0151] 1% by weight Fixative 1
[0152] 5% weight percentage binder 3
[0153] 1% Wetting agent 5
[0154] 0.25% by weight defoamer 1
[0155] 10% by weight Moisturizer 1
[0156] 66.55% by weight Water Viscosity: 2,3 mPa·s pH: 8.1
[0157] Change in viscosity after the test period: +0.1 mPa·s Change in pH after the test period: -0.2 Redispersibility of sediment after the test period: Yes Change in particle size after the test period: Acceptable Example 9
[0158] 15% by weight Pigment 2
[0159] 1.2% by weight Dispersant 1
[0160] 1% by weight Fixative 1
[0161] 5% weight percentage binder 6
[0162] 3% Wetting agent 5
[0163] 0.25% by weight defoamer 1
[0164] 10% by weight Moisturizer 1
[0165] 64.55% by weight water
[0166] Viscosity: 5.1 mPa·s
[0167] pH: 8.1
[0168] Change in viscosity after the test period: Undetermined Change in pH after the test period: -0.3
[0169] Redispersibility of sediment after test period: Yes Change in particle size after test period: Acceptable Comparative Example 1
[0170] 15% by weight Pigment 1
[0171] 1.5% by weight Dispersant 1
[0172] 1% by weight Fixative 1
[0173] 5% weight percentage binder 8
[0174] 0.25% by weight defoamer 1
[0175] 10% by weight Moisturizer 1
[0176] 67.25% by weight water
[0177] Viscosity: 11.6 mPa·s
[0178] pH: 8.4
[0179] Change in viscosity after the test period: +12.9 mPa·s Change in pH after the test period: -0.3 Redispersible sediment after the test period: no sediment Change in particle size after the test period: polydisperse mixture Comparative Example 2
[0180] 15% by weight Pigment 2
[0181] 1.5% by weight Dispersant 2
[0182] 5% weight percentage binder 7
[0183] 5% weight percentage binder 3
[0184] 0.25% by weight defoamer 1
[0185] 10% by weight Moisturizer 1
[0186] 63.25% by weight Water Viscosity: 8.5 mPa·s pH: 8.2
[0187] Viscosity change after test period: -0.8 mPa·s pH change after test period: -0.4 Redispersible sediment after test period: Yes Particle size change after test period: Unacceptable Comparative Example 3
[0188] 15% by weight Pigment 1
[0189] 1.2% by weight Dispersant 1
[0190] 1% by weight Fixative 1
[0191] 5% weight percentage binder 9
[0192] 0.25% by weight defoamer 1
[0193] 10% by weight Moisturizer 1
[0194] 67.55% by weight Water Viscosity: 5 mPa·s
[0195] pH: 8.4
[0196] Change in viscosity after the test period: +3.2 mPa·s Change in pH after the test period: -2,1 Redispersibility of sediment after the test period: yes Change in particle size after the test period: unacceptable
Claims
1. An inkjet ink comprising the following components: a) at least one pigment; b) at least one dispersant having an acid number of less than 20 mg KOH / g based on the total dispersant; c) at least one fixing agent selected from multivalent calcium salts, wherein the amount of the at least one fixing agent is in the range of 0.05% to 1% by weight with respect to the total inkjet ink; d) at least one binder selected from polyurethanes having an acid value of less than 20 mg KOH / g based on the total binder; and e) water; in, The inkjet ink has a viscosity of less than 30 mPa·s as measured by a cone and plate viscometer at 25° C., Therein, the at least one binder d) is selected from nonionic and anionic polyurethanes.
2. The inkjet ink according to claim 1, in, The inkjet ink has a viscosity of less than 20 mPa·s as measured by a cone and plate viscometer at 25°C.
3. The inkjet ink according to claim 1, in, The at least one fixing agent c) is selected from calcium chloride, calcium acetate, calcium nitrate and mixtures thereof.
4. The inkjet ink according to claim 3, in, The at least one fixing agent c) is calcium chloride.
5. The inkjet ink according to any one of the preceding claims 1 to 4, in, The amount of the at least one binder d) is in the range of 1 to 20% by weight, based on the total inkjet ink.
6. The inkjet ink according to any one of the preceding claims 1 to 4, in, The amount of the at least one dispersant b) is in the range of 0.1 to 10% by weight, based on the total inkjet ink.
7. The inkjet ink according to any one of the preceding claims 1 to 4, in, The amount of the at least one pigment a) is in the range of 1 to 30% by weight, based on the total inkjet ink.
8. The inkjet ink according to any one of the preceding claims 1 to 4, in, The at least one pigment a) is selected from white pigments.
9. The inkjet ink according to any one of the preceding claims 1 to 4, in, The amount of water e) is in the range of 30 to 90% by weight based on the total inkjet ink.
10. The inkjet ink according to claim 1, in, The inkjet ink has a viscosity of less than 10 mPa·s as measured by a cone and plate viscometer at 25°C.
11. A printing method, wherein The following steps are involved: i) providing a printing substrate; ii) inkjet printing at least one inkjet ink according to any one of claims 1 to 10 onto a printing substrate; iii) drying the inkjet ink printed in step ii); iv) inkjet printing at least one additional inkjet ink onto the inkjet ink dried in step iii); v) Drying the further inkjet ink printed in step iv).
12. The printing method according to claim 11, wherein the drying in steps iii) and v) is performed by heating.
13. The printing method according to claim 11 or 12, in, The printing substrate has a water absorption capacity of less than 10 g water / kg printing substrate.
14. The printing method according to claim 11 or 12, in, In step ii), printing is performed on a plastic surface, a metal surface or a combination thereof.
Citation Information
Patent Citations
White pre-treatment composition
EP2718110A1
Aqueous paint composition
EP3798276A1
Inkjet receptive compositions and methods therefor
US20170321084A1
Aqueous inkjet ink
WO2007035505A1
Fluid set for textile printing
WO2020046341A1