Amorphous coating and preparation method thereof

By using cold spraying technology to prepare iron-based amorphous coating on metal surfaces such as aluminum alloys and magnesium alloys, the problem of difficulty in preparing protective films with high density in the prior art is solved, and high hardness, wear resistance, Improved corrosion resistance and magnetic permeability reduce costs and avoid crystallization and oxidation problems.

CN116463622BActive Publication Date: 2024-11-05UV TECH MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310349569.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-11-05
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

The prior art is difficult to prepare protective films with thicker surfaces and high structural density on metal alloys such as aluminum alloys and magnesium alloys, which makes it difficult to meet the performance requirements of aviation, aerospace and other equipment. High temperatures in thermal spraying process can easily lead to crystallization or oxidation of the amorphous coating, reducing performance.

Method used

The iron-based amorphous coating is prepared on the surface of the matrix such as aluminum alloy and magnesium alloy by cold spraying. By controlling process parameters such as injection pressure, temperature and injection distance, amorphous coating is used for alloy elements such as Fe, Cr, Mo, Si, B. Alloy powder, prepare amorphous coating with low oxidation degree and dense structure.

Benefits of technology

It significantly improves the hardness, wear resistance and corrosion resistance of the amorphous coating, and reduces costs, avoids crystallization and oxidation problems in the thermal spraying process, and achieves high density and good magnetic permeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116463622B_ABST
    Figure CN116463622B_ABST
Patent Text Reader

Abstract

The present invention relates to an amorphous coating and a preparation method thereof. The amorphous coating is composed of an iron-based alloy, and in addition to Fe and Cr elements, it also contains a variety of main elements of Si, B, P, C, Al, and Mo, as well as a small amount of one or more alloying elements of Ni, Zr, Nb, Y, etc. By selecting a suitable element ratio, the amorphous coating can have good hardness, wear resistance, corrosion resistance and thermal stability. The amorphous coating is sprayed and deposited on the surface of a substrate by a high-pressure cold spraying process. In addition to having the characteristics of low oxidation degree, good structural density, and not easy to fall off, the amorphous coating of the present invention also has the beneficial effects of improving the hardness, wear resistance, corrosion resistance, magnetism, etc. of the coating. The present invention also relates to a preparation method for a corrosion-resistant amorphous coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of amorphous coatings, and in particular to an amorphous coating and a preparation method thereof. Background Art

[0002] Nonferrous metals such as aluminum alloys, magnesium alloys, and copper alloys are widely used in industrial products, but these materials are not ideal due to their active chemical properties, wear resistance, and corrosion resistance. At present, electroplating, anodizing, micro-arc oxidation, laser surface treatment, coating, etc. are generally used to prepare protective functional films or fine-grained and nanocrystalline structures on the surfaces of these metal materials to improve the wear resistance and corrosion resistance of the surfaces of these metal alloy products. However, these processes are difficult to prepare thicker films with high structural density, so it is difficult to meet the performance requirements of many aviation, aerospace, weapons, and other equipment. By selecting some powder materials with good wear resistance and corrosion resistance (such as oxides such as aluminum oxide, zirconium oxide, and chromium oxide, or amorphous materials such as iron-based amorphous alloys and nickel-based amorphous alloys), combined with thermal spraying or cold spraying processes, a layer of protective coating with high structural density and thick thickness is sprayed and deposited on the surface of some metal workpieces with high surface performance requirements, which can significantly improve the surface hardness, wear resistance, and corrosion resistance of the product, and even give the workpiece surface good special functions such as good heat insulation, magnetic conductivity, and wave absorption.

[0003] Amorphous alloys have the characteristics of high hardness, high strength, high wear resistance, and high corrosion resistance. Coatings prepared with amorphous alloys can significantly improve the surface properties of the substrate. At present, amorphous alloy coatings suitable for protective functions mainly include Ni-based coatings and Fe-based coating systems, but the cost of Ni-based coatings is high, which is not conducive to practical promotion and application. Fe-based amorphous alloy coatings have high cost performance and good wear resistance and corrosion resistance, and are suitable as surface protective coating materials for engineering structural parts. At present, thermal spraying technology, such as arc spraying and plasma spraying, is generally used to prepare iron-based amorphous coatings. However, due to the high heating temperature (2500~10000℃) during the thermal spraying construction process, high temperature can easily cause the prepared amorphous coating to crystallize or even oxidize, reducing the inherent properties of amorphous alloys; in addition, coatings prepared by thermal spraying often have problems such as high porosity (>5%) and poor bonding strength.

[0004] Cold spraying mainly uses high-pressure, high-speed heated gas to provide deposition power for metal powders. When the powder exceeds a certain critical speed, it will hit the substrate surface at high speed, causing shear and rheology of the powder material, and then deposit on the substrate surface, gradually achieving stacking and forming, and realizing the preparation of the coating. Since the gas used in the cold spraying construction process is basically protective, such as nitrogen, argon, etc., and the gas heating temperature is relatively low (300~1200℃), when spraying amorphous metal powder, the amorphous powder is not prone to oxidation or crystallization, so it is suitable for the preparation of iron-based amorphous alloy coatings.

[0005] At the same time, the density, hardness and corrosion resistance of the coatings prepared by the existing process are difficult to coordinate and improve, and the performance of the products is prone to vary, thus affecting the efficiency of product use. Summary of the invention

[0006] In view of the defects of the prior art, the purpose of the present invention is to provide an amorphous coating and a preparation method thereof to solve the problems raised in the above background technology.

[0007] The present invention solves the technical problem by adopting the following technical solution:

[0008] The invention provides an amorphous coating with a compact structure, which is sprayed on the surface of a substrate as a layered coating. The amorphous coating is made by a cold spraying process, and the porosity of the coating is 0.5-2.0%.

[0009] By using cold spraying technology, a layer of highly dense amorphous coating is prepared on the substrates of aluminum alloy, magnesium alloy, copper alloy, etc. to achieve good surface wear resistance, corrosion resistance and other properties. Amorphous alloy fine powder mainly composed of alloy elements such as Fe, Cr, Mo, Si, B, Al, etc. is used as raw material. By controlling the process parameters of cold spraying, an iron-based amorphous coating with low oxidation degree, dense structure and good bonding strength is prepared, which can significantly improve the performance of aluminum alloy, magnesium alloy, copper alloy, etc., and obtain good coating hardness, wear resistance, corrosion resistance and other properties.

[0010] The density, wear resistance, corrosion resistance and other properties of the amorphous coating prepared on the metal surface by this cold spraying technology are significantly better than those of the amorphous coating prepared by thermal spraying, and are also significantly better than those of the pure iron coating prepared by cold spraying.

[0011] Cold spraying, also known as gas dynamic spraying technology, refers to a method in which metal particles are accelerated to a certain critical speed, and after the particles collide with the substrate, they undergo strong plastic deformation and deposit to form a metal coating. Under normal conditions, the general concept is that when solid particles collide with a certain substrate, the solid particles will erode the substrate.

[0012] The beneficial effects of the present invention are as follows: the iron-based amorphous coating has the characteristics of low oxidation degree, good structural density, not easy to fall off, and relatively low price, and has the beneficial effects of improving the hardness, wear resistance, corrosion resistance, and magnetic conductivity of the surface of the base metal.

[0013] Furthermore, the porosity of the amorphous coating is 0.5 to 2.0%.

[0014] The beneficial effect of adopting the above technical solution is that it can improve the wear resistance and corrosion resistance of the iron-based amorphous coating. Below this range, the process will be difficult to implement; above this range, the hardness, wear resistance and corrosion resistance of the amorphous magnetic conductive coating will decrease.

[0015] Furthermore, the thickness of the amorphous coating is 0.1-0.25 mm.

[0016] The beneficial effects of adopting the above technical solution are: it helps to improve the hardness, wear resistance, corrosion resistance and magnetic conductivity of the amorphous coating. Below this range, the amorphous coating will be too thin, the protective performance will be insufficient and it will be difficult to construct; above this range, the surface roughness and structural density of the amorphous coating will deteriorate, and the processing and preparation costs will be significantly increased.

[0017] Furthermore, the amorphous coating uses iron-based amorphous alloy powder as a matrix material, the powder is spherical or nearly spherical, and the sphericity of the powder is ≥0.85.

[0018] The beneficial effects of adopting the above technical solution are: iron-based amorphous alloy powder with high sphericity is beneficial to improving the deposition efficiency of the coating and reducing the porosity of the coating. Low sphericity will lead to a decrease in the deposition efficiency of the coating, an increase in the porosity inside the coating, and a deterioration in the hardness, wear resistance, corrosion resistance and electromagnetic heating effect of the coating.

[0019] Furthermore, the powder particle size of the iron-based amorphous alloy is 1000-400 meshes.

[0020] The beneficial effects of adopting the above technical solution are: using amorphous alloy powder with smaller particle size is conducive to improving the deposition efficiency of the amorphous coating, and improving the density, wear resistance and corrosion resistance of the coating. If the powder particle size is too small, it is easy to cause powder agglomeration; if the powder particle size is too high, it is easy to cause the deposition efficiency and density of the amorphous alloy coating to decrease, and the hardness, wear resistance, corrosion resistance and magnetic conductivity of the amorphous coating will deteriorate.

[0021] Furthermore, the composition of the amorphous coating is an iron-based amorphous alloy, which contains at least two or more alloying elements of Si, B, P, C, Al, and Mo in addition to the two main elements of Fe and Cr. The atomic fraction (at.%) of each element is in the range of 5%≤Si≤15%, 10%≤B≤15%, 4%≤C≤8%, 5%≤P≤10%, 2%≤Al≤5%, and 2%≤Mo≤5%, respectively, which can promote the amorphous alloy to have good wear resistance, corrosion resistance, and magnetic properties. Among them, if the Fe content is too low, the hardness of the powder will be high, which is not conducive to the deposition of the coating, and the magnetic conductivity of the obtained amorphous coating will decrease. If the Fe content is too high, the hardness and wear resistance of the amorphous alloy coating will decrease. If the Cr content is too low, the wear resistance and corrosion resistance of the amorphous coating will decrease. If the Cr content is too low, the hardness of the amorphous alloy powder will be too high, and the cold spray deposition efficiency will decrease.

[0022] Furthermore, the amorphous coating composition is an iron-based amorphous alloy, which, in addition to the above-mentioned alloying elements, also contains a small amount of one or more elements such as Ni, Zr, Nb, Y, etc., and the atomic fraction (at.%) of these elements is preferably in the range of: 1%≤Ni≤3.5%, 0.2%≤Zr≤1%, 0.2%≤Nb≤1%, 0.2%≤Y≤1%.

[0023] The beneficial effect of adopting the above technical solution is that the iron-based amorphous alloy contains one or more of the elements such as Zr, Nb, Ni, and Y at a low content, which can significantly improve the thermal stability of the amorphous alloy, inhibit the crystallization problem caused by gas heating during the cold spraying process of the substrate, and ensure that the performance of the prepared amorphous coating does not show a significant decline. If the content of the added element is too low, the effect of improving the thermal stability of the amorphous alloy is not obvious, and if the content of the added element is too high, the thermal stability of the amorphous alloy will also decrease.

[0024] The present invention solves the above-mentioned other technical problem with the following technical solution: a method for preparing a dense amorphous coating, comprising the following steps: cold spraying iron-based amorphous alloy powder on the surface of the structure to be sprayed by using a working gas.

[0025] Furthermore, the working gas is one or more of nitrogen and argon.

[0026] The beneficial effect of adopting the above technical solution is that both nitrogen and argon can provide a good protective atmosphere. During the preparation process of the amorphous coating, they have the effect of protecting the substrate powder of the amorphous coating from being basically oxidized, and as a protective gas, they also have a good cost advantage.

[0027] Furthermore, the spraying pressure of the cold spraying is 4-10 Mpa.

[0028] The beneficial effects of adopting the above technical solution are: adopting the above pressure is conducive to ensuring that the amorphous coating has a higher speed and deposition power, the packaging coating has good bonding strength and density, and the wear resistance and corrosion resistance of the coating are improved; if the pressure is too low, it will lead to a low injection rate of the metal powder, a decrease in the coating deposition efficiency, and poor wear resistance and corrosion resistance of the coating; if the pressure is too high, it will cause the cold spray process to be difficult to control.

[0029] Furthermore, the spraying temperature of the cold spraying (heating temperature of the spraying gas) is 500-850°C.

[0030] The beneficial effects of adopting the above technical scheme are: adopting the above-mentioned gas heating temperature is conducive to reducing the degree of oxidation and crystallization of the spray powder when it is subjected to the action of high-temperature gas, improving the fluidity, deposition efficiency and bonding strength of the powder, and improving the performance of the amorphous coating; if the gas temperature is too high, the powder will be subjected to excessive thermal action of the high-temperature gas, which will easily lead to more oxidation and crystallization problems, thereby reducing the performance of the amorphous coating; if the temperature is too low, it will lead to problems such as poor bonding strength and density of the amorphous coating.

[0031] Furthermore, the spraying distance of the cold spraying is 5 to 20 mm.

[0032] The beneficial effect of adopting the above technical solution is that when the cold spray powder reaches the surface of the workpiece for deposition, it has a sufficiently high flight speed to ensure a good deposition effect, improve the density, wear resistance and corrosion resistance of the coating. If the spray distance is too large, the deposition effect of the spray powder will be poor, and the density, wear resistance and corrosion resistance of the coating will be poor. If the spray distance is too small, the cold spray process will be difficult to control.

[0033] Preferably, after the cold spraying process is completed, a modification liquid is used for impregnation modification treatment, and after the impregnation is completed, the surface is washed with water, dried, and modified by thermal optimization. The temperature of the thermal optimization modification is 120-130°C, and the temperature is kept for 10-15 minutes, and then cooled to room temperature at a rate of 1-3°C / min.

[0034] The impregnation pressure of the impregnation modification is 10-15MPa, and the impregnation time is 20-30min;

[0035] The preparation method of the modified liquid is:

[0036] The bentonite is sent to 300-350℃ for heat treatment for 20-30min, then cooled to 55-60℃ at a rate of 2-5℃ / min, and then placed in 4-6 times the mass fraction of 5% hydrochloric acid solution for primary stirring modification;

[0037] Subsequently, 6% chitosan aqueous solution, 1-3% lanthanum sulfate and 0.2-0.5% silane coupling agent KH560 are added to the mixture in an amount of 2-5% of the total amount of the hydrochloric acid solution, and the mixture is subjected to secondary stirring modification. After the stirring is completed, a modified solution is obtained.

[0038] Preferably, the rotation speed of the first-stage stirring modification is 800-1000 r / min, and the stirring time is 30-40 min. The rotation speed of the second-stage stirring modification is 350-450 r / min, and the stirring time is 55-65 min.

[0039] Through the impregnation modification treatment and then the thermal optimization modification, the modifying liquid in the impregnation modification uses bentonite that has been heat-treated to optimize the interlamellar spacing, and then the primary modification and stirring of the hydrochloric acid solution is used to improve the dispersibility of the bentonite. In combination with the secondary stirring treatment of chitosan aqueous solution, lanthanum sulfate and silane coupling agent KH560, the mixing degree of the raw materials in the modified liquid is improved. At the same time, after the thermal modification, the performance effect of the coating is more coordinated.

[0040] Preferably, the deposition carrier of the amorphous coating is made of non-ferrous metals such as aluminum alloy, magnesium alloy, titanium alloy and copper alloy.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] The present invention adopts a cold spraying process to spray and prepare an iron-based amorphous coating with high hardness, high strength, high wear resistance and high corrosion resistance on the surface of the base material, and also has good magnetic conductivity, which can significantly improve the comprehensive surface performance of workpieces such as aluminum alloys, magnesium alloys, and copper alloys. By adopting cold spraying technology, a layer of high-density amorphous coating is prepared on the substrates of materials such as aluminum alloys, magnesium alloys, and copper alloys to achieve good surface wear resistance, corrosion resistance and other properties. The thickness range of the amorphous coating is conducive to ensuring that the amorphous coating has a good surface strengthening effect and improves production efficiency. If the thickness is too high, it will lead to problems such as high surface roughness of the coating, decreased coating density, and high processing costs; if the thickness is too low, it will lead to problems such as insufficient protection performance and electromagnetic heating performance of the amorphous coating. Aluminum alloys, magnesium alloys, copper alloys, titanium alloys, etc. all have poor surface hardness, wear resistance, corrosion resistance and other properties, and basically have no magnetic conductivity. After preparing iron-based amorphous coatings on their surfaces, the properties of the amorphous coatings themselves can be used to significantly improve the surface hardness, wear resistance, and corrosion resistance of the substrate, and give the substrate good magnetic properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a schematic diagram of the amorphous coating structure of the present invention.

[0044] Figure 2 The corrosion resistance test results of the amorphous coatings of the embodiments and comparative examples are shown in FIG.

[0045] In the accompanying drawings, the components represented by the reference numerals are listed as follows:

[0046] 1. Substrate, 2. Amorphous coating. Implementation

[0047] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] The present invention is an amorphous coating, which is composed of an iron-based amorphous alloy, containing two main elements, Fe and Cr, and their atomic fractions (at.%) range respectively: 45% ≤ Fe ≤ 70%, 10% ≤ Cr ≤ 20%; in addition, it also contains at least two or more alloying elements of Si, B, P, C, Al, and Mo, and the atomic fractions (at.%) of each element range respectively: 5% ≤ Si ≤ 15%, 10% ≤ B ≤ 15%, 4% ≤ C ≤ 8%, 5% ≤ P ≤ 10%, 2% ≤ Al ≤ 5%, 2% ≤ Mo ≤ 5%. In addition to the above-mentioned alloying elements, it also contains a small amount of one or more elements such as Ni, Zr, Nb, and Y, and the atomic fractions (at.%) of these elements preferably range: 1% ≤ Ni ≤ 3.5%, 0.2% ≤ Zr ≤ 1%, 0.2% ≤ Nb ≤ 1%, and 0.2% ≤ Y ≤ 1%.

[0049] The amorphous magnetic conductive coating is sprayed on the surface of the substrate by cold spraying, and the porosity of the amorphous coating is 0.5-2.0%. Preferably, the porosity of the amorphous coating is 0.7-1.5%, and the thickness is 0.1-0.2 mm.

[0050] The invention also discloses a method for preparing an amorphous coating, comprising the following steps: cold spraying iron-based amorphous alloy powder onto the surface of a structure to be sprayed by using a working gas.

[0051] The working gas is one or more of argon and nitrogen. The spray pressure of the cold spray is 4-10 MPa. The spray temperature of the cold spray is 500-850°C, and the spray distance of the cold spray is 10-30 mm. The powder particle size of the magnetic conductive metal is 1000-400 mesh. The thickness of the magnetic conductive coating is 0.1-0.2 mm.

[0052] Furthermore, the above process conditions can also be: the working gas is one or more of argon and nitrogen. The spray pressure of the cold spray is 5-8 MPa. The spray temperature of the cold spray is 550-700°C, and the spray distance of the cold spray is 10-20 mm. The sphericity of the amorphous alloy powder is ≥0.95, and the powder particle size is 1000-600 mesh. The thickness of the magnetic conductive coating is 0.1-0.2 mm. The porosity of the amorphous coating is 0.8-1.5%.

[0053] An amorphous coating, the amorphous coating is located on the surface of a metal substrate. The substrate is made of aluminum alloy, magnesium alloy, titanium alloy, copper alloy, etc. The wear resistance of the amorphous coating is fed back through Vickers hardness, because the wear resistance of a general metal is positively correlated with its hardness. The average hardness value of the cross section of the amorphous coating is tested by a Vickers hardness tester as the final hardness value of the coating. The corrosion resistance of the amorphous coating is tested by an electrochemical workstation in a NaCl solution with a mass fraction of 3.5% at room temperature. The corrosion resistance of the coating is judged by the measured corrosion current density value of the film layer sample.

[0054] The following is a detailed introduction through some specific embodiments.

[0055] Using a cold spray system, compressed nitrogen accelerates the iron-based amorphous alloy powder, which is then sprayed through a nozzle onto the surface of the substrate and physically deformed. The iron-based amorphous alloy powder is embedded in the outer surface of the metal substrate and firmly attached, and then deposited layer by layer to form a layer of iron-based amorphous alloy with good density, which gives the substrate good hardness, wear resistance, corrosion resistance, and magnetic conductivity.

[0056] Example 1

[0057] An amorphous coating is provided, wherein the amorphous coating is located on the outer surface of a metal substrate. The substrate is made of 7075 aluminum alloy. The amorphous coating is prepared on the surface of the aluminum alloy by cold spraying process, comprising the following steps:

[0058] 1. Degrease the surface of the aluminum alloy substrate;

[0059] 2. The amorphous alloy powder is cold sprayed on the surface of the 7075 aluminum alloy by the working gas nitrogen. The amorphous alloy powder is deposited on the surface of the substrate at a high speed to form an amorphous coating. The specific process parameters are:

[0060] (1) The cold sprayed powder is Fe52Cr15Si8B14C6Al2Mo2Zr0.5Nb0.5 iron-based amorphous alloy powder with a purity of not less than 99.5%, and the atomic fractions (at.%) of Fe, Cr, Si, B, C, Al, Mo, Z, and Nb are 52, 15, 8, 14, 6, 2, 2, 0.5, and 0.5, respectively; the powder sphericity is about 0.9, and the powder particle size is 800-500 mesh; the working gas used is high-purity nitrogen with a purity of 99.9%; the injection pressure is 5-6 MPa; the spraying distance is 15-20 mm; the spraying temperature (i.e., the gas heating temperature) is 600-700 °C, and the thickness of the prepared amorphous coating is 0.1-0.2 mm.

[0061] Example 2

[0062] An amorphous coating is provided, wherein the amorphous coating is located on the surface of a metal substrate. The material of the metal substrate is 2024 aluminum alloy. The iron-based amorphous coating is prepared on the surface of the aluminum alloy by a cold spraying process, comprising the following steps:

[0063] 1. Degrease the surface of the aluminum alloy substrate;

[0064] 2. Cold spraying the iron-based amorphous alloy powder on the surface of 2024 aluminum alloy by heated working gas nitrogen, the iron-based amorphous alloy powder is deposited on the surface of the substrate at a high speed to form an iron-based amorphous coating, and the specific process parameters are:

[0065] The amorphous alloy powder adopts Fe49Cr18Si8B14C6Al2Mo2Zr0.5Y0.5 iron-based amorphous alloy powder with a purity of not less than 99.5%, a powder sphericity of about 0.9, and a powder particle size of 600-400 meshes; the working gas adopts high-purity nitrogen with a purity of 99.9%; the injection pressure is 5-6 Mpa; the spraying distance is 15-20 mm; the spraying temperature (i.e., the gas heating temperature) is 600-700 ° C. The thickness of the prepared amorphous coating is 0.15-0.25 mm.

[0066] Example 3

[0067] An amorphous coating is provided, wherein the amorphous coating is located on the surface of a metal substrate. The material of the metal substrate is H80 (Al-Sn) copper alloy. The iron-based amorphous coating is prepared on the surface of the copper alloy by a cold spraying process, comprising the following steps:

[0068] 1. Sandblast the surface of H80 copper alloy to be sprayed, and the surface roughness reaches 2~4 μm;

[0069] 2. The amorphous alloy powder is cold sprayed on the surface of the copper alloy by heated working gas argon. The amorphous alloy powder is deposited on the surface of the copper alloy at a high speed to form an iron-based amorphous coating. The specific process parameters are:

[0070] The amorphous alloy powder adopts Fe52Cr15Si8B14C6Al2Mo2Ni1.5Nb0.5 iron-based amorphous alloy powder with a purity of not less than 99.5%, the iron-based amorphous alloy powder, the powder sphericity is ≥0.9, and the powder particle size is 800-500 mesh; the working gas adopts high-purity argon with a purity of 99.9%, the injection pressure is 7-8 Mpa, the spraying distance is 15-20 mm; the spraying temperature (i.e., the gas heating temperature) is 600-700 ° C. The thickness of the prepared amorphous coating is 0.1-0.2 mm.

[0071] Example 4

[0072] An amorphous coating is provided, wherein the amorphous coating is located on the surface of a metal substrate. The material of the technical substrate is AZ31 magnesium alloy. The iron-based amorphous coating is prepared on the surface of the magnesium alloy by cold spraying process, comprising the following steps:

[0073] 1. Degreasing the surface of magnesium alloy;

[0074] 2. The amorphous alloy powder is cold sprayed on the surface of the magnesium alloy by heated working gas nitrogen. The amorphous alloy powder is deposited at a high speed on the surface of the magnesium alloy to form an iron-based amorphous coating. The specific process parameters are:

[0075] The magnetic conductive powder is selected from Fe52Cr15Si8B14C6Al2Mo2Zr0.5Nb0.5 iron-based metal powder with a purity of not less than 99.5%, a powder sphericity of ≥0.9, and a particle size of 800-500 meshes; the purity of the high-purity argon gas used as the working gas is 99.9%; the injection pressure is 7-8 Mpa, the spraying distance is 10-15 mm; the spraying temperature (i.e., the gas heating temperature) is 600-700°C. The thickness of the prepared amorphous coating is 0.1-0.2 mm.

[0076] Example 5

[0077] An amorphous coating is provided, wherein the amorphous coating is located on the outer surface of a metal substrate. The substrate is made of 7075 aluminum alloy. The amorphous coating is prepared on the surface of the aluminum alloy by cold spraying process, comprising the following steps:

[0078] 1. Degrease the surface of the aluminum alloy substrate;

[0079] 2. The amorphous alloy powder is cold sprayed on the surface of the 7075 aluminum alloy by the working gas nitrogen. The amorphous alloy powder is deposited on the surface of the substrate at a high speed to form an amorphous coating. The specific process parameters are:

[0080] The cold sprayed powder is Fe52Cr15Si8B14C6Al2Mo2Zr0.5Nb0.5 iron-based amorphous alloy powder with a purity of not less than 99.5%, a powder sphericity of about 0.9, and a powder particle size of 800-500 meshes; the working gas uses high-purity nitrogen with a purity of 99.9%; the spray pressure is 5-6 Mpa; the spray distance is 15-20 mm; the spray temperature (i.e., gas heating temperature) is 550-650 ° C. The thickness of the prepared amorphous coating is 0.1-0.2 mm.

[0081] Comparative Example 1

[0082] On the basis of Example 1, the composition of the sprayed amorphous alloy material was adjusted, and the iron-based amorphous alloy powder used was Fe43Cr24Si8B14C6Al2Mo2Zr0.5Nb0.5 (atomic mass fraction), and the rest was the same as Example 1.

[0083] Comparative Example 2

[0084] On the basis of Example 1, the composition of the sprayed amorphous alloy material was adjusted, and the iron-based amorphous alloy powder used was Fe60Cr7Si8B14C6Al2Mo2Zr0.5Nb0.5 (atomic mass fraction), and the rest was the same as Example 1.

[0085] Comparative Example 3

[0086] On the basis of Example 1, the spraying temperature (ie, the gas heating temperature) was adjusted to 900-1000° C., and the rest was the same as Example 1.

[0087] Comparative Example 4

[0088] On the basis of Example 1, the injection pressure was adjusted to 2-3 MPa, and the rest was the same as Example 1.

[0089] Comparative Example 5

[0090] On the basis of Example 1, the spray distance was adjusted to 40-45 mm, and the rest was the same as Example 1.

[0091] The porosity, microhardness and corrosion resistance of the coatings obtained in each embodiment and each comparative example are respectively tested below. The performance test results of each coating are shown in Table 1.

[0092] Table 1

[0093] name Coating porosity / % Average coating hardness / HV Corrosion current density icorr / μA·cm-2 Example 1 1.09 1590 5.38 Example 2 1.15 1560 5.84 Example 3 0.84 1630 4.41 Example 4 0.80 1500 3.76 Example 5 1.24 1550 6.15 Comparative Example 1 1.05 1640 4.92 Comparative Example 2 0.96 1470 4.75 Comparative Example 3 0.85 1610 4.54 Comparative Example 4 3.30 1130 9.83 Comparative Example 5 2.40 1340 8.56

[0094] According to the data in Table 1, it can be seen that by strictly controlling the process parameters of cold spraying, a layer of amorphous coating with high density, high hardness, high wear resistance, high corrosion resistance and high magnetic conductivity can be prepared on the surface of non-ferrous metal materials such as aluminum alloy, magnesium alloy and copper alloy. The raw material of the amorphous coating is fine powder of iron-based amorphous alloy. The iron-based amorphous alloy mainly contains two alloy elements, Fe and Cr, and their atomic fraction (at.%) ranges are: 45%≤Fe≤70%, 10%≤Cr≤20%; in addition, it also contains at least two or more alloy elements of Si, B, P, C, Al and Mo, and the atomic fraction (at.%) ranges are: 5%≤Si≤15%, 10%≤B≤15%, 4%≤C≤8%, 5%≤P≤10%, 2%≤Al≤5%, 2%≤Mo≤5%. In addition to the above alloying elements, it also contains a small amount of one or more elements such as Ni, Zr, Nb, and Y, and the atomic fraction (at.%) of these elements is preferably in the range of: 1%≤Ni≤3.5%, 0.2%≤Zr≤1%, 0.2%≤Nb≤1%, 0.2%≤Y≤1%. The preferred amorphous coating is characterized by a coating thickness of 0.1-0.2 mm and a coating porosity of 0.6-1.5%.

[0095] The present invention further optimizes the process based on Example 3:

[0096] Optimization example 1:

[0097] On the basis of Example 3, after the cold spraying process is completed, a modification liquid impregnation modification treatment is also used. After the impregnation is completed, the surface is washed with water and dried. The surface is modified by thermal optimization. The temperature of the thermal optimization modification is 125°C, and the surface is kept warm for 12 minutes, and then cooled to room temperature at a rate of 2°C / min.

[0098] The impregnation pressure of the impregnation modification was 12MPa and the impregnation time was 25min;

[0099] The preparation method of the modified liquid is:

[0100] The bentonite was heat treated at 325°C for 25 min, then cooled to 58°C at a rate of 3.5°C / min, and then placed in a 5-fold mass fraction 5% hydrochloric acid solution for primary stirring modification;

[0101] Subsequently, 6% chitosan aqueous solution, 2% lanthanum sulfate and 0.35% silane coupling agent KH560 were added with a total amount of 3.5% of the hydrochloric acid solution, and secondary stirring modification was performed. After the stirring was completed, a modified solution was obtained.

[0102] The speed of the first-stage stirring modification is 900 r / min, and the stirring time is 35 min. The speed of the second-stage stirring modification is 400 r / min, and the stirring time is 60 min.

[0103] Comparative Optimization Example 1

[0104] The only difference from Optimization Example 1 is that no thermal optimization modification was used after the cold spraying process.

[0105] Comparative Optimization Example 2

[0106] The only difference from Optimization Example 1 is that no modification liquid immersion modification is used after the cold spraying process.

[0107] Comparative Optimization Example 3

[0108] The only difference from Optimization Example 1 is that the modified liquid preparation method is different: bentonite is replaced by graphene.

[0109] Comparative Optimization Example 4

[0110] The only difference from Optimization Example 1 is that the preparation method of the modified liquid is different: no chitosan aqueous solution is added.

[0111] Optimization Example 1, Comparative Example The test results of optimization examples 1-4 are shown in Table 2

[0112] Table 2

[0113] name Coating porosity / % Average coating hardness / HV Corrosion current density icorr / μA·cm-2 Optimization Example 1 0.64 1695 3.25 Comparative Optimization Example 1 0.73 1652 4.12 Comparative Optimization Example 2 0.78 1643 4.25 Comparative Optimization Example 3 0.75 1651 4.02 Comparative Optimization Example 4 0.71 1658 3.98

[0114] From Optimization Example 1, it can be seen that after the cold spray process, the modifying liquid immersion modification treatment is also adopted. After the immersion, water washing and drying, through thermal optimization modification, the product's coating porosity, coating average hardness and corrosion current density performance all show coordinated improvement effects. At the same time, after the cold spray process, if neither thermal optimization modification nor modifying liquid immersion modification is adopted, and the modifying liquid preparation method is different, the product performance shows a trend of deterioration. Only by using thermal optimization modification and modifying liquid immersion modification treatment in coordination, the two can synergize and enhance the performance of the product.

[0115] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0116] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. An amorphous coating, characterized in that: The composition of the amorphous coating is an iron-based amorphous alloy containing Fe and Cr elements in a stoichiometric ratio, and the amorphous coating is made by depositing iron-based amorphous metal powder on the surface of the substrate through high-speed air pressure spraying; The amorphous coating is made by cold spraying process, the porosity of the amorphous coating is 0.5-2.0%, and the thickness is 0.1-0.25 mm; After the cold spraying process is completed, a modification liquid is used for impregnation modification. After the impregnation is completed, the material is washed with water and dried. The thermal optimization modification is performed at a temperature of 120-130°C, and the temperature is kept at 10-15 minutes. The material is then cooled to room temperature at a rate of 1-3°C / min. The impregnation pressure of the impregnation modification is 10-15MPa, and the impregnation time is 20-30min; The preparation method of the modified liquid is: The bentonite is sent to 300-350℃ for heat treatment for 20-30min, then cooled to 55-60℃ at a rate of 2-5℃ / min, and then placed in 4-6 times the mass fraction of 5% hydrochloric acid solution for primary stirring modification; Then, 2-5% of the total amount of the hydrochloric acid solution, 6% chitosan aqueous solution, 1-3% lanthanum sulfate and 0.2-0.5% silane coupling agent KH560 were added, and the mixture was subjected to secondary stirring modification. After the stirring was completed, a modified solution was obtained. The atomic fraction (at.%) of Fe and Cr in the iron-based non-gold alloy is in the range of 45%≤Fe≤70%, 10%≤Cr≤20%; it also contains at least two or more alloying elements of Si, B, P, C, Al, and Mo, and the atomic fraction (at.%) of each element is in the range of 5%≤Si≤15%, 10%≤B≤15%, 4%≤C≤8%, 5%≤P≤10%, 2%≤Al≤5%, 2%≤Mo≤5%; The iron-based non-gold alloy also contains one or more elements such as Ni, Zr, Nb, and Y that can improve the thermal stability of the amorphous alloy and are not easy to crystallize during the cold spraying process. The atomic fraction (at.%) of the stability element ranges from 1%≤Ni≤3.5%, 0.2%≤Zr≤1%, 0.2%≤Nb≤1%, 0.2%≤Y≤1%; The working gas heating temperature of the cold spraying is 500-850°C; The spraying pressure of the cold spraying is 4 to 10 MPa; The spraying distance of the cold spraying is 5 to 20 mm.

2. The amorphous coating according to claim 1, characterized in that: The shape of the amorphous alloy powder material used for cold spraying is spherical or nearly spherical, the powder sphericity is ≥0.85, and the powder particle size is 1000-400 meshes.

3. The amorphous coating according to claim 1, characterized in that: The working gas for cold spraying is one or a mixed protective gas of nitrogen and argon.

4. The amorphous coating according to claim 1, characterized in that: The rotation speed of the first-stage stirring modification is 800-1000r / min, and the stirring time is 30-40min. The rotation speed of the second-stage stirring modification is 350-450r / min, and the stirring time is 55-65min.

5. The amorphous coating according to claim 1, characterized in that: The deposition carrier of the amorphous coating is made of non-ferrous metals such as aluminum alloy, magnesium alloy, titanium alloy and copper alloy.