A Cu-based catalyst for water-gas shift reaction and preparation method thereof

By introducing Al3+ elements into the CuFe2O4 precursor, the CuAlxFe2-xO4 catalyst was solved, and the stability and activity of CuFe2O4 catalyst in low-temperature water gas transformation reaction was achieved, more efficient catalytic performance and thermal stability were achieved, and CO conversion was significantly improved. rate and service life.

CN116474775BActive Publication Date: 2024-11-01FUZHOU UNIV

Patent Information

Application Number
CN202310321951.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-11-01
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

The CuFe2O4 precursor catalyst has problems of insufficient stability and activity in the low-temperature water gas transformation reaction, which leads to its inactivation at high temperatures and affects the catalytic performance.

Method used

CuFe2O4 is partially replaced by introducing Al3+ elements, and CuAlxFe2-xO4 precursor is prepared, and Cu-based catalyst is obtained through reduction treatment. Al3+ is used as a structural additive to prevent particles from growing, increasing specific surface area and active sites, and improving the catalyst Thermal stability and activity.

Benefits of technology

It significantly improves the water-gas transformation reaction activity and thermal stability of the catalyst, increases the specific surface area and Cu nanoparticle size, improves the synergistic effect between active components and carriers, and achieves more efficient CO conversion and longer use. life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116474775B_ABST
    Figure CN116474775B_ABST
Patent Text Reader

Abstract

The present invention discloses a Cu-based catalyst for water-gas shift reaction and a preparation method thereof. The method adopts a sol-gel method and uses citric acid as a complexing agent to make Cu 2+ 、Al 3+ with Fe 3+ The CuAl is uniformly mixed at the molecular level, and then gelled, dried and calcined at high temperature to obtain CuAl x Fe 2‑x O4 precursor, and then reduced to obtain a supported Cu-based catalyst. The present invention introduces the element Al to perform B-site doping modification on CuFe2O4 to prepare a spinel-type composite oxide precursor, which promotes the synergistic effect between the metal-carrier in the reduction product, reduces the activation energy of the water-gas shift reaction, and thus exhibits excellent catalytic activity and thermal stability of the water-gas shift reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalyst preparation and heterogeneous catalysis, and particularly relates to a supported Cu-based catalyst for water-gas shift reaction and a preparation method thereof. Background Art

[0002] Hydrogen is a potential clean fuel energy source that has attracted widespread attention due to its high energy efficiency and wide resource sources. At present, most hydrogen is produced from traditional fossil fuels, and the water-gas shift reaction (WGS, CO+H2O→CO2+H2, ΔH=-41.1 kJ / mol) is one of the key steps in industrial hydrogen production. In this process, catalysts are one of the keys to improving reaction efficiency and economic benefits.

[0003] The water-gas shift reaction is an exothermic reaction, and low temperature is conducive to the forward reaction. Due to the high cost of precious metals, existing research has increasingly focused on the development of non-precious metal catalysts. Therefore, Cu-based catalysts with good water-gas shift reaction performance at low temperatures have been widely studied. Chinese patent CN 106378141A discloses a method for preparing a ZnO / Cu nanocrystalline composite material, which is a cube and an octahedron, and its activity is compared with that of Cu nanocrystals, showing extremely high catalytic performance. Budiman et al. (Budiman, A.et al. Appl. Catal.A: Gen. 2013,462-463,220) reported a highly dispersed Cu / ZnO / Al2O3 catalyst prepared by an improved coprecipitation method. Chinese patent CN111482179A introduces additives Zr, Zn, Ca, K and Mg into the Cu / Al2O3 catalyst to obtain a low-temperature Cu-based shift catalyst with good low-temperature activity, high yield, large specific surface area, good heat resistance, good aging resistance and long service life. Kameoka et al. (Kameoka, S.et al. Catal. Lett.2005, 100, 89) found that spinel CuFe2O4 is an efficient copper-based catalyst precursor. Lin et al. (Lin, XYet al. Acta Phys. Chim. Sin. 2014, 30, 157) studied Cu / Fe2O3 catalysts with different Cu loadings and found that spinel structured CuFe2O4 plays an important role in improving catalytic activity. However, for Cu catalysts with CuFe2O4 as precursor, Cu microcrystals are prone to agglomeration and deactivation, so the stability and activity of the catalyst need to be improved. To this end, the present invention provides a preparation method that can improve catalytic performance based on the B-site doping modification of the CuFe2O4 precursor to obtain a Cu-based catalyst with high activity and stability. Summary of the invention

[0004] The object of the present invention is to provide a high-performance non-precious metal spinel oxide-supported Cu-based catalyst having excellent catalytic activity for water-gas shift reaction.

[0005] To achieve the above purpose, the present invention adopts the following technical steps:

[0006] A Cu-based catalyst for water-gas shift reaction, which is AB2O4 spinel-type composite oxide CuAl x Fe 2-x O4 (x is 0.25~1) is used as a precursor, and the supported Cu catalyst is obtained by reduction.

[0007] The preparation method of the Cu-based catalyst comprises the following steps:

[0008] (1) Mix copper salt, iron salt and aluminum salt in proportion, add to deionized water, stir at 25-60°C for 1-4 hours, then add citric acid and mix well, and stir at 50-70°C for 1-4 hours to form a sol;

[0009] (2) Raise the system temperature to 80-100°C and continue stirring until a gel is formed;

[0010] (3) The gel obtained in step (2) is dried and calcined to obtain CuAl x Fe 2-x O4 precursor;

[0011] (4) The CuAl obtained in step (3) x Fe 2-x The Cu-based catalyst was prepared by reducing the O4 precursor.

[0012] Furthermore, the amount of copper salt, iron salt and aluminum salt used is based on Cu 2+ with (Fe 3+ +Al 3+ ) is converted in a molar ratio of 1:2, and Al 3+ with Fe 3+ The molar ratio is x:(2-x), where x=0.25-1.

[0013] Furthermore, the copper salt includes one or more of copper nitrate, copper acetate, copper chloride and copper sulfate.

[0014] Furthermore, the iron salt includes one or more of ferric nitrate, ferric chloride and ferric sulfate.

[0015] Furthermore, the aluminum salt includes one or more of aluminum nitrate, aluminum chloride, and aluminum sulfate.

[0016] Furthermore, the ratio of the molar amount of citric acid used to the total molar amount of the metal salt is (1.5-2.5):1.

[0017] Furthermore, in step (3), the drying temperature is 140-170°C and the time is 3-8 h; the calcination temperature is 600-900°C (heating rate is 2°C / min) and the time is 1-6 h.

[0018] Furthermore, the reduction in step (4) is carried out in an atmosphere of 5 vol.% H2 / N2 at 200-300°C for 2-4h.

[0019] The technical solution of the present invention has the following advantages:

[0020] The present invention provides a Cu-based water-gas shift catalyst, which is 3+ Fe in CuFe2O4 3+ Partial substitution was performed to prepare CuAl x Fe 2-x O4 precursor, the specific surface area of ​​the precursor is significantly larger than that of the unmodified sample, and the use of Al 3+ As a structural additive, it prevents particle growth and stabilizes the carrier. The Cu nanoparticles in the Cu-based catalyst obtained after reduction are smaller in size, which increases the number of active sites on the surface. At the same time, there is a good synergistic effect between the active components and the carrier, thereby improving the activity and thermal stability of the water-gas shift reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The XRD graphs of the catalyst precursors obtained in Example 2, Example 3, Example 4 and Comparative Example 1 (A) and their XRD graphs after reduction at 250°C (B) are shown in the figure. 3+ Compared with Comparative Example 1, Examples 2-4 produced purer spinel oxides with better crystallinity. The peaks of Examples 2-4 shifted to the right as a whole, indicating that Al 3+ Successfully replaced Fe 3+ Entered the catalyst.

[0022] Figure 2 The H2-TPR graphs of the catalyst precursors obtained in Example 2, Example 3, Example 4 and Comparative Example 1. As can be seen from the graph, compared with Comparative Example 1, the reduction temperatures of the catalyst samples obtained in Examples 2-4 are lower, indicating that there is a good synergistic effect between the metal and the carrier.

[0023] Figure 3The activity (a) and stability (b) of the catalyst precursors obtained in Example 2, Example 3, Example 4 and Comparative Example 1 after reduction at 250°C are compared. As can be seen from the figure, the CO conversion rates of the catalyst sample of Example 2 at 240°C, 280°C and 320°C are 80.8%, 78.1% and 72.8% respectively, the CO conversion rates of the catalyst sample of Example 3 at 240°C, 280°C and 320°C are 80.5%, 78.3% and 71.2% respectively, the CO conversion rates of the catalyst sample of Example 4 at 240°C, 280°C and 320°C are 79.2%, 72.0% and 68.9% respectively, and the CO conversion rates of the catalyst sample of Comparative Example 1 at 240°C, 280°C and 320°C are 43.9%, 63.2% and 64.7% respectively. It can be seen that the activities of Examples 2 and 3 are much greater than the activity of Comparative Example 1. In the second performance test, the activity of each catalyst sample decreased in the following order: Example 3 < Example 4 < Example 2 < Comparative Example 1, so Example 3 has the best thermal stability and activity. DETAILED DESCRIPTION

[0024] A Cu-based catalyst for water-gas shift reaction, the preparation method of which comprises the following steps:

[0025] (1) Mix copper salt, iron salt and aluminum salt in proportion, add to deionized water, stir at 25-60°C for 1-4 hours, then add citric acid and mix well, and stir at 50-70°C for 1-4 hours to form a sol;

[0026] (2) Raise the system temperature to 80-100°C and continue stirring until a gel is formed;

[0027] (3) The gel obtained in step (2) is dried at 140-170°C for 3-8 h, and then calcined at 600-900°C for 1-6 h to obtain CuAl x Fe 2-x O4 precursor;

[0028] (4) The CuAl obtained in step (3) x Fe 2-x The O4 precursor was treated in a reducing atmosphere of 5 vol.% H2 / N2 at 200-300 °C for 2-4 h to obtain a Cu-based catalyst.

[0029] The amount of copper salt, iron salt and aluminum salt used is based on Cu 2+ with (Fe 3+ +Al 3+ ) is converted in a molar ratio of 1:2, and Al 3+ with Fe 3+ The molar ratio is x:(2-x), x=0.25-1.

[0030] The copper salt includes one or more of copper nitrate, copper acetate, copper chloride and copper sulfate.

[0031] The iron salt includes one or more of ferric nitrate, ferric chloride and ferric sulfate.

[0032] The aluminum salt includes one or more of aluminum nitrate, aluminum chloride and aluminum sulfate.

[0033] The ratio of the molar amount of the citric acid used to the total molar amount of the metal salt is (1.5-2.5):1.

[0034] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.

[0035] Embodiment 1:

[0036] 0.033 mol Cu(NO3)2·3H2O, 0.00825 mol Al(NO3)3·9H2O and 0.0578 mol Fe(NO3)3·9H2O were accurately weighed and added into 600 mL of deionized water to completely dissolve them. The mixed salt solution was then heated to 65°C and stirred for 4 h. 0.1683 mol monohydrated citric acid (C6H8O7·H2O) was then added and kept for 1 h to form a sol. The system temperature was then raised to 95°C and stirred until gelation. The obtained gel was dried at 150°C for 4 h and lightly ground, and then calcined at 650°C for 2 h (heating rate 2°C / min) in static air to obtain Cu(Al) 0.25 Fe 1.75 O4 catalyst precursor.

[0037] Embodiment 2:

[0038] 0.033 mol Cu(NO3)2·3H2O, 0.0165 mol Al(NO3)3·9H2O and 0.0495 mol Fe(NO3)3·9H2O were accurately weighed and added into 600 mL of deionized water to completely dissolve them. The mixed salt solution was then heated to 65°C and stirred for 4 h. 0.1683 mol monohydrated citric acid (C6H8O7·H2O) was then added and kept for 1 h to form a sol. The system temperature was then raised to 95°C and stirred until gelation. The obtained gel was dried at 150°C for 4 h and lightly ground, and then calcined at 650°C for 2 h (heating rate 2°C / min) in static air to obtain Cu(Al) 0.5 Fe 1.5 O4 catalyst precursor.

[0039] Embodiment 3:

[0040] 0.033 mol Cu(NO3)2·3H2O, 0.0248 mol Al(NO3)3·9H2O and 0.0413 mol Fe(NO3)3·9H2O were accurately weighed and added into 600 mL of deionized water to completely dissolve them. The mixed salt solution was then heated to 65°C and stirred for 4 h. 0.1683 mol monohydrated citric acid (C6H8O7·H2O) was then added and kept for 1 h to form a sol. The system temperature was then raised to 95°C and stirred until gelation. The obtained gel was dried at 150°C for 4 h and lightly ground, and then calcined at 650°C for 2 h (heating rate 2°C / min) in static air to obtain Cu(Al) 0.75 Fe 1.25 O4 catalyst precursor.

[0041] Embodiment 4:

[0042] Accurately weigh 0.033 mol Cu(NO3)2·3H2O, 0.033 mol Al(NO3)3·9H2O and 0.033 mol Fe(NO3)3·9H2O, add them into 600 mL of deionized water to completely dissolve them, then heat the mixed salt solution to 65°C and stir for 4 h, then add 0.1683 mol citric acid monohydrate (C6H8O7·H2O) and keep it for 1 h to form a sol; then raise the system temperature to 95°C and continue stirring until gelation; the obtained gel is dried at 150°C for 4 h and lightly ground, then calcined at 650°C for 2 h (heating rate 2°C / min) in static air to obtain a Cu(Al)FeO4 catalyst precursor.

[0043] Comparative Example 1:

[0044] Accurately weigh 0.033 mol Cu(NO3)2·3H2O and 0.066 mol Fe(NO3)3·9H2O, add them into 600 mL of deionized water to completely dissolve them, then heat the mixed salt solution to 65°C, stir for 4 h, add 0.1683 mol citric acid monohydrate (C6H8O7·H2O) and keep it for 1 h to form a sol; then raise the system temperature to 95°C, continue stirring until gelation; the obtained gel is dried at 150°C for 4 h and lightly ground, then calcined at 650°C for 2 h (heating rate 2°C / min) in static air to obtain a CuFeO4 catalyst precursor.

[0045] Table 1 Textural properties of different catalyst precursors and the grain size of Cu in the catalysts

[0046]

[0047] It can be seen from Table 1 that compared with Comparative Example 1, Examples 2-4 have larger specific surface areas and pore volumes, among which Example 3 has the largest specific surface area; and from the most probable pore diameter, it can be seen that the examples are mainly mesoporous structures, indicating that Al 3+ The introduction of can increase the specific surface area of ​​the catalyst precursor and change the pore structure of the precursor. At the same time, compared with comparative example 1, examples 2-4 have smaller Cu species grain sizes, indicating that Al 3+ The introduction of helps to inhibit the growth of Cu particles.

[0048] Comparative Example 2:

[0049] Accurately weigh 0.033 mol Cu(NO3)2·3H2O, 0.033 mol Cr(NO3)3·9H2O and 0.033 mol Fe(NO3)3·9H2O, add them into 600 mL of deionized water to completely dissolve them, then heat the mixed salt solution to 65°C and stir for 4 h, then add 0.1683 mol citric acid monohydrate (C6H8O7·H2O) and keep it for 1 h to form a sol; then raise the system temperature to 95°C and continue stirring until gelation; the obtained gel is dried at 150°C for 4 h and lightly ground, then calcined at 650°C for 2 h (heating rate 2°C / min) in static air to obtain Cu(Cr)FeO4 catalyst precursor.

[0050] Comparative Example 3:

[0051] Accurately weigh 0.033 mol Cu(NO3)2·3H2O, 0.033 mol Ce(NO3)3·9H2O and 0.033 mol Fe(NO3)3·9H2O, add them into 600 mL of deionized water to completely dissolve them, then heat the mixed salt solution to 65°C and stir for 4 h, then add 0.1683 mol citric acid monohydrate (C6H8O7·H2O) and keep it for 1 h to form a sol; then raise the system temperature to 95°C and continue stirring until gelation; the obtained gel is dried at 150°C for 4 h and lightly ground, then calcined at 650°C for 2 h (heating rate 2°C / min) in static air to obtain Cu(Ce)FeO4 catalyst precursor.

[0052] Catalyst performance evaluation

[0053] 1 g (40-60 mesh) of the catalyst precursors prepared in Examples 1-4 and Comparative Examples 1-3 were weighed respectively, and the catalyst precursors were reduced in a fixed bed reactor with a stainless steel tube with an inner diameter of 12 mm (reduction temperature was 250°C, reduction time was 2-4 h, and reduction atmosphere was 5 vol.% H2 / N2). The activity of the obtained catalysts in the water-gas shift reaction was evaluated in the temperature range of 200-400°C, and the reaction conditions were: mass space velocity was 9000 h -1 The raw gas composition is 15 vol. % CO, 55 vol. % H2, 7 vol. % 12CO2 and 23 vol. % N2, and the gas-steam ratio is 4:1. The test results are shown in Table 1.

[0054] Table 2 Comparison of the activity of different catalysts in water-gas shift reaction

[0055]

[0056] As can be seen from Table 2, compared with the undoped Al comparative example 1, the CO conversion rates of the catalyst samples obtained in Examples 1-4 doped with Al are significantly improved, among which Example 3 has the best CO conversion rate. Compared with Comparative Examples 2 and 3 doped with other metals, the CO conversion rates of the catalyst samples doped with Al in Examples 1-4 are significantly higher, which effectively shows that the Al-modified catalyst has a better water-gas shift reaction performance.

[0057] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A Cu-based catalyst for water-gas shift reaction, characterized in that: The catalyst is prepared by accurately weighing 0.033 mol Cu(NO3)2·3H2O, 0.0248 mol Al(NO3)3·9H2O and 0.0413 mol Fe(NO3)3·9H2O, adding them into 600 mL of deionized water to completely dissolve them, then heating the mixed salt solution to 65°C, stirring for 4 hours, adding 0.1683 mol monohydrated citric acid and keeping it for 1 hour to form a sol; then raising the system temperature to 95°C, and continuing to stir until gelling; drying the obtained gel at 150°C for 4 hours and lightly grinding it, and then calcining it at 650°C for 2 hours in static air at a heating rate of 2°C / min to obtain Cu(Al) 0.75 Fe 1.25 O4 catalyst precursor.

Citation Information

Patent Citations

  • ZnO / Cu nanometer crystal composite material, and preparation method and application thereof

    CN106378141A

  • Low-temperature Cu-series shift catalyst as well as preparation method and application thereof

    CN111482179A

  • Iron-based water gas transformation catalyst and preparation method thereof

    CN102350355A

  • Heatproof Cu / ZnAl2O4 low temperature water gas converting catalyst

    CN105214671A

  • Regeneration method of copper / ferroferric oxide water-gas conversion catalyst

    CN107754815A

Cited By

  • Copper-iron supported catalyst for water gas shift reaction and preparation method thereof

    CN118059920A

  • Copper-iron supported catalysts for water-gas shift reaction and their preparation method

    CN118059920B