A mesoporous catalyst coating with flower-like clusters and a catalyst prepared therefrom

By using a mesoporous catalyst with a flower-like cluster structure in the catalyst coating, combined with modified γ-Al2O3 and porous ceramic carrier, the problems of uneven catalyst coating structure and complex coating preparation are solved, and the catalytic performance and economic benefits are improved. , simplifies the process flow and is suitable for industrial production.

CN116474800BActive Publication Date: 2024-10-22UNIV OF JINAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310411735.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-22
Estimated Expiration
2043-04-12

AI Technical Summary

Technical Problem

Existing catalyst coatings have problems such as high particle agglomeration, uneven pore size structure, loss of active sites, complex coating preparation, high cost, multiple roasting times, and high energy consumption, resulting in low catalytic performance and high economic costs.

Method used

A mesoporous catalyst coating with flower-like clusters is used. By modifying γ-Al2O3 and porous ceramic carrier, combined with the co-catalytic component and the main catalytic component, a multi-step impregnation and one-time roasting process is used to form a three-dimensional network pore size. Structure and flower-like clusters, reduce coating thickness and raw material costs, and improve active phase utilization.

Benefits of technology

It achieves a uniformly dispersed pore structure, improves gas flow channels, increases specific surface area, improves catalytic performance, reduces raw material costs and energy consumption, simplifies the process flow, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116474800B_ABST
    Figure CN116474800B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of catalyst technology, and specifically relates to a mesoporous catalyst coating with flower-like clusters and a catalyst prepared therefrom. The coating comprises a modified component and a main catalytic component; the modified component comprises γ-Al2O3 modified by non-metallic elements and variable-valence metal oxides or other alkaline earth and rare earth metal oxides with abundant active sites; the main catalytic component is a metal oxide with a certain high-efficiency catalytic effect. The coating composition conversion is completed by using a multi-step impregnation and one-time roasting method, and nitrates and ammonia water corresponding to multi-metal oxides are used to realize the combination of coating synthesis and coating deposition process. The ammonium radical and weak acid radical are used to regulate the morphology of nano-alumina to obtain flower-like clusters, so that the coating has uniform mesopores and a large number of gas channels. Compared with direct oxide coating, the cost of raw materials is reduced, there is no need to consider spray curing, the synthesized coating is thinner, the time and economic cost are lower, and the energy consumption is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and in particular relates to a mesoporous catalyst coating with flower-like clusters and a catalyst prepared therefrom. Background Art

[0002] Monolithic catalysts are widely used in organic waste gas treatment, water pollution purification, photocatalysis and other fields due to their controllable structure and excellent fluid dynamics. They are mainly composed of porous monolithic carriers and active coatings. At present, the addition of active coatings is mainly done by direct spraying or dipping the coating and then baking. Among them, direct spraying is not only difficult to control the uniformity, but also requires a large amount of materials, and may require multiple spraying. The use of the dipping-baking method also needs to face the challenges of complex processes such as carrier pretreatment, advance deposition of binder coatings, multiple depositions, and multiple baking. For example, CN114985937A pre-treats the carrier with sandblasting and then sprays the prepared oxide powder, and the resulting coating is thicker; CN115025778A, CN113969069A, etc. all need to add a bonding coating or add a binder to the coating to ensure coating adhesion; the coatings deposited by CN11222149613A and CN102133537A include a porous base coating and a main catalytic coating, which require multiple baking. Based on the optimization of the number of calcinations, patent CN108889309A achieves single coating and single calcination, but the coating mixing makes part of the active phase easy to be coated by other oxides, and a binder still needs to be added to assist bonding.

[0003] Most importantly, existing coatings generally have a phenomenon of highly agglomerated particles, resulting in a large loss of active sites, uneven dispersion of pore structures, blocked gas channels, and low utilization of active phases, which significantly reduces the advantages of coatings. Secondly, the above processes are similar to CN113584417A, which directly uses the target oxide as a raw material, or similar to RU2017117114220, which uses oxides and metal particles prepared in advance with metal salts and metal bases as coatings, that is, the preparation of the coating and the deposition of the coating are two processes. This means that the economic and time costs required for the coating are high and the dosage is large. Summary of the invention

[0004] There are three problems at this stage: (1) Due to the high agglomeration of coating particles, there is a lack of gas flow channels, the pore structure is randomly uneven, the specific surface area is small, and a large number of active sites are lost. (2) The synthesis of the coating and the coating deposition process are separated, resulting in high cost of active oxide coating raw materials, complicated coating preparation steps, complex coating deposition process, and too thick deposited coating. (3) The carrier pretreatment requirements are high, multiple roastings are energy-intensive and time-consuming, and an additional bonding coating needs to be sprayed or a binder needs to be added to the coating.

[0005] The technical solution of the present invention is:

[0006] A mesoporous catalyst coating with flower-like clusters comprises a modified component and a main catalytic component;

[0007] The modified component includes a modified porous component and a catalytic promoter component;

[0008] The modified porous component is γ-Al2O3 modified by non-metallic elements;

[0009] The co-catalyst component is a variable valence metal oxide or other alkaline earth metal or rare earth metal oxide with abundant oxygen vacancies and active sites;

[0010] The main catalytic component is a metal oxide having a high-efficiency catalytic effect on a certain reaction.

[0011] Preferably, the non-metallic element of the non-metallic element-modified γ-Al2O3 is P, B or Si; and / or the co-catalyst component is CeO2, MgO, BaO; and / or the main catalytic component is Pd, Pt, Ru, Cu or Ni.

[0012] Preferably, it comprises the above-mentioned mesoporous catalyst coating with flower-like clusters and a porous carrier.

[0013] Preferably, the porous carrier is porous ceramic; the porous ceramic is honeycomb ceramic or foam ceramic.

[0014] Preferably, the mesoporous catalyst coating having flower-like clusters accounts for 1-6 wt % of the entire catalyst.

[0015] Another object of the present invention is to provide a method for preparing the above-mentioned mesoporous catalyst having flower-like clusters, comprising the following steps:

[0016] (1) preparing aluminum nitrate and nitrate corresponding to the co-catalyst component into a hot nitrate solution at 70-90° C., which is the impregnation solution L1;

[0017] (2) adding a weak acid corresponding to the non-metallic element dropwise into 50-90° C. ammonia water and ultrasonically preparing an ammonia water immersion liquid L2 in which a weak acid ammonium salt is dissolved;

[0018] (3) adding the nitrate corresponding to the main catalytic component dropwise into ammonia water and ultrasonically preparing an immersion solution L3;

[0019] (4) After cleaning the porous ceramic, place it in the impregnation liquid L1, blow air to remove the residual impregnation liquid, and dry it; at this time, a nitrate coating is obtained; then place it in the impregnation liquid L2, seal it and let it stand, and dry it; at this time, the nitrate coating is transformed into an alkaline coating adsorbed with ammonium ions and weak acid ions; finally place it in the impregnation liquid L3; heat it in a water bath and dry it; at this time, the alkaline coating is combined with the ammonium nitrate salt corresponding to the main catalytic element;

[0020] (5) The porous ceramic that has completed the impregnation step is calcined at 300-700° C. for 3-6 hours to synthesize the multi-oxide catalytic coating.

[0021] Preferably, the nitrate content corresponding to the co-catalytic component in step (1) is 5%-30wt%; the aluminum nitrate content is 30-60wt%.

[0022] Preferably, the concentration of the aqueous ammonia used in steps (1) and (2) is above 22 wt %;

[0023] Preferably, in step (2), the mass ratio of the weak acid corresponding to the non-metallic element to the mass ratio of the ammonia water impregnation solution L2 in which the weak acid ammonium salt is dissolved is 0.1-5wt%.

[0024] Preferably, the mass of the nitrate corresponding to the main catalytic component in step (3) is calculated by converting the main catalytic element to 0.01%-1% of the mass of the porous ceramic.

[0025] The nitrate coating used in the present invention after impregnation L1 is mainly aluminum nitrate, and after impregnation L2, the aluminum nitrate becomes aluminum hydroxide, and is combined with ammonium radicals and weak acid radicals (modified non-metallic elements), which play a role in regulating the morphology. In the last step of calcination, aluminum hydroxide becomes γ-alumina, ammonium radicals become ammonia, and weak acid radicals remain to play a modifying role; the mesoporous catalytic coating with flower-like clusters prepared in this application has a three-dimensional mesh aperture structure, and part of the nano-alumina on the surface of the coating is agglomerated into pine needle-like leaves, which are gathered at one end and assembled into flower-like clusters with radial structures.

[0026] Beneficial effects of the present invention:

[0027] (1) After multiple composition changes, the coating finally obtains a uniformly dispersed mesh pore size and mesoporous structure, and weak acid salts and ammonia water adjust the surface of nano-alumina to form flower-like clusters. These special morphologies provide a large number of flow channels for the reaction gas, transporting the gas to every corner of the coating, giving full play to the advantages of the coating and improving the mass transfer efficiency. The special structure of the coating increases the specific surface area, releases the active sites, increases the utilization rate of the active phase, and improves the catalytic performance.

[0028] (2) Using nitrates and ammonia water corresponding to multi-metal oxides, the porous oxide, the catalytic oxide and the catalytic active phase are prepared at the same time, realizing the combination of coating synthesis and coating deposition process. Compared with direct oxide coating, the cost of raw materials is reduced, there is no need to consider spray curing, and the synthesized coating is thinner. In addition, due to the use of a multi-step impregnation and a single calcination method, the time and economic costs are low and the energy consumption is reduced.

[0029] (3) There is no need to perform additional treatment on the carrier in advance, spray viscous materials to assist the coating in bonding, or add additional adhesives to the coating, and the coating is stable and not easy to fall off.

[0030] (4) This technology is simple to operate, uses simple raw materials, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The three-dimensional mesh pores and flower-like clusters formed by nano-alumina particles on the coating surface (left); the flower-like clusters are widely distributed in the coating (right);

[0032] Figure 2 The pore size comparison between the coating produced by this process (left picture) and the common coating (right picture) obtained by nitrogen physical adsorption and desorption test;

[0033] Figure 3 This is the XRD pattern of the catalyst prepared in Example 3.

[0034] Example 1

[0035] A method for preparing a mesoporous catalyst having flower-like clusters comprises the following steps:

[0036] (1) Dissolve 6 kg of aluminum nitrate and 2 kg of cerium nitrate in 10 L of deionized water and heat to 80° C. in a water bath to obtain the impregnation solution L1;

[0037] (2) 0.076 kg of 85 wt% phosphoric acid was added dropwise to 9.1 kg of 25 wt% ammonia water at 60° C. and ultrasonicated for 10 min; this was the immersion solution L2;

[0038] (3) 1 kg of 4 wt% palladium nitrate solution was added dropwise to 1 kg of 25 wt% ammonia solution and ultrasonicated for 10 min; this was the impregnation solution L3;

[0039] (4) The volume density of 1 kg is 1 g / cm 3 After cleaning, the honeycomb ceramic is placed in the impregnation liquid L1 for 120 seconds, the residual impregnation liquid is removed by blowing, and it is taken out and dried at 70°C for 2 hours to obtain a nitrate coating; it is then placed in the impregnation liquid L2 and sealed and allowed to stand for 30 minutes, and it is taken out and dried at 80°C for 3 hours, and the nitrate coating is converted into an alkaline coating adsorbed with ammonia and phosphate; finally, it is placed in the impregnation liquid L3, heated in a water bath at 70°C for 40 minutes, and the impregnation liquid and the ceramic are dried at 110°C for 6 hours to obtain an alkaline coating combined with palladium salt;

[0040] (5) The honeycomb ceramic described in step (4) is calcined at 550° C. for 4 hours to obtain a multi-oxide mesoporous catalyst containing flower-like alumina clusters.

[0041] Example 2

[0042] A method for preparing a mesoporous catalyst having flower-like clusters comprises the following steps:

[0043] (1) Dissolve 6.5 kg of aluminum nitrate and 1.8 kg of barium nitrate in 10 L of deionized water and heat to 70° C. in a water bath to obtain the impregnation solution L1;

[0044] (2) 2.15 kg of 3 wt% boric acid was added dropwise to 9 kg of 25 wt% ammonia water at 50° C. and ultrasonicated for 5 min; this was the immersion solution L2;

[0045] (3) 0.75 kg of 4 wt% palladium nitrate solution was added dropwise to 1 kg of 25 wt% ammonia solution and ultrasonicated for 8 min; this was the impregnation solution L3;

[0046] (4) The volume density of 1 kg is 1 g / cm 3 The honeycomb ceramic is cleaned and placed in the impregnation liquid L1 for 60 seconds, and then taken out and blown to remove the residual impregnation liquid, and dried at 80°C for 2 hours to obtain a nitrate coating; then placed in the impregnation liquid L2 and sealed and allowed to stand for 60 minutes, and then taken out and dried at 80°C for 4 hours, and the nitrate coating is converted into an alkaline coating adsorbed with ammonia and borate; finally placed in the impregnation liquid L3, heated in a water bath at 70°C for 30 minutes, and the impregnation liquid and ceramic are dried at 100°C for 8 hours to obtain an alkaline coating combined with palladium salt;

[0047] (5) The porous ceramic described in step (4) is calcined at 550° C. for 5 h to obtain a multi-oxide mesoporous catalyst containing flower-like alumina clusters.

[0048] Example 3

[0049] A method for preparing a mesoporous catalyst having flower-like clusters comprises the following steps:

[0050] (1) Dissolve 7 kg of aluminum nitrate and 4 kg of cerium nitrate in 10 L of deionized water and heat to 70° C. in a water bath to obtain the impregnation solution L1;

[0051] (2) 0.085 kg of 85 wt% phosphoric acid was added dropwise to 9.5 kg of 25 wt% ammonia water at 70° C. and ultrasonicated for 8 min; this was the immersion solution L2;

[0052] (3) 1.25 kg of 4 wt% ruthenium nitrate solution was added dropwise to 1 kg of 25 wt% ammonia solution and ultrasonicated for 6 min; this was the impregnation solution L3;

[0053] (4) The volume density of 1 kg is 1 g / cm 3The foam ceramic was cleaned and placed in the impregnation liquid L1 for 100 seconds, and the residual impregnation liquid was removed by blowing. After being taken out, it was dried at 60°C for 3 hours to obtain a nitrate coating; it was then placed in the impregnation liquid L2 and sealed and allowed to stand for 40 minutes. After being taken out, it was dried at 80°C for 3 hours, and the nitrate coating was converted into an alkaline coating adsorbed with ammonia and phosphate; finally, it was placed in the impregnation liquid L3, heated in a water bath at 70°C for 50 minutes, and the impregnation liquid and ceramic were dried at 120°C for 4 hours to obtain an alkaline coating combined with ruthenium salt;

[0054] (5) calcining the foam ceramic described in step (4) at 500° C. for 6 h to obtain a multi-oxide mesoporous catalyst containing flower-like alumina clusters.

[0055] from Figure 3 It can be seen that the coating on the porous ceramic of the present application is γ-Al2O3.

[0056] Implementation effect example

[0057] The catalytic activity of the catalysts of Examples 1-3 was investigated, taking CO2 methanation and CO oxidation as examples to examine the catalytic performance.

[0058] Experimental conditions:

[0059] The CO2 methanation reaction was completed in a micro-catalytic activity evaluation system with a power of 2500W. 50mg of the catalyst was placed in a quartz tube with an inner diameter of 6mm for reaction. The volume ratio of CO2, H2, and N2 was 8:32:60, and the investigation temperature was 350℃. The tail gas was detected by a mass spectrometer and a gas chromatograph.

[0060] The CO oxidation reaction was carried out in a quartz tube fixed bed reactor with an inner diameter of 6 mm at atmospheric pressure, and the inlet and outlet gases were detected by gas chromatograph. The catalyst was 50 mg, the reaction gas was 10% O2, 1% CO and 89% N2, and the total flow rate was 50 mL min -1 A thermocouple was inserted in the center of the catalyst to control the investigation temperature of the catalyst in the device to be 130°C.

[0061] The investigation time for CO2 methanation and CO oxidation reactions was 60 days.

[0062] The specific results are shown in Table 1.

[0063] Table 1 Experimental results

[0064]

Claims

1. A mesoporous catalyst with flower-like clusters, It is characterized in that It comprises a mesoporous catalyst coating with flower-like clusters and a porous carrier, wherein the mesoporous catalyst coating comprises a modified component and a main catalytic component; the porous carrier is a porous ceramic; The modified component includes a modified porous component and a catalytic promoter component; the modified porous component is a γ-Al modified by a non-metallic element. 2 O 3 The co-catalyst component is a variable valence metal oxide or other alkaline earth metal or rare earth metal oxide with abundant oxygen vacancies and active sites; the main catalytic component is a CO 2 Metal oxides with high catalytic activity in methanation or CO oxidation reactions; The preparation method of the mesoporous catalyst comprises the following steps: (1) Aluminum nitrate and nitrate corresponding to the co-catalyst component are prepared into a hot nitrate solution at 70-90° C., which is the impregnation solution L1; (2) adding a weak acid corresponding to the non-metallic element dropwise into ammonia water at 50-90°C and ultrasonically preparing an ammonia water immersion solution L2 in which a weak acid ammonium salt is dissolved; (3) Add the nitrate corresponding to the main catalytic component dropwise into ammonia water and ultrasonically prepare an impregnation solution L3; (4) After cleaning the porous ceramic, place it in the impregnation liquid L1, blow air to remove the residual impregnation liquid, and dry it; at this time, a nitrate coating is obtained; then place it in the impregnation liquid L2, seal it and let it stand, and dry it; at this time, the nitrate coating is transformed into an alkaline coating adsorbed with ammonium ions and weak acid ions; finally place it in the impregnation liquid L3; heat it in a water bath and dry it; at this time, the alkaline coating is combined with the ammonium nitrate salt corresponding to the main catalytic element; (5) The porous ceramic that has completed the impregnation step is calcined at 300-700 °C for 3-6 h to synthesize the multi-oxide catalytic coating.

2. The mesoporous catalyst having flower-like clusters according to claim 1, Characterized by non-metal Element-modified γ-Al 2 O 3 The non-metallic element is P, B or Si; and / or the co-catalyst component is CeO 2 , MgO, BaO; and / or the main catalytic component is an oxide of Pd, Pt, Ru, Cu or Ni.

3. The mesoporous catalyst having flower-like clusters according to claim 1, It is characterized in that The porous ceramic is honeycomb ceramic or foam ceramic.

4. The mesoporous catalyst having flower-like clusters according to claim 1, It is characterized in that The mesoporous catalyst coating with flower-like clusters accounts for 1-6 wt% of the entire catalyst.

5. The mesoporous catalyst having flower-like clusters according to claim 1, It is characterized in that In the step (1), the nitrate content corresponding to the co-catalyst component is 5-30 wt%; the aluminum nitrate content is 30-60 wt%.

6. The mesoporous catalyst having flower-like clusters according to claim 1, It is characterized in that The concentration of the aqueous ammonia used in steps (1) and (2) is above 22 wt%.

7. The mesoporous catalyst having flower-like clusters according to claim 1, It is characterized in that In the step (2), the mass ratio of the weak acid corresponding to the non-metallic element to the mass ratio of the ammonia water impregnation solution L2 in which the weak acid ammonium salt is dissolved is 0.1-5 wt%.