A supported heteropolyacid catalyst for high-selective synthesis of glutaraldehyde by cyclopentene oxidation and its application
By loading quaternary ammonium salt and phosphotungstic acid on the silica substrate, the supported phosphotungsten heteropolyacid catalyst is solved, and the existing catalyst efficiency and recovery difficulties are achieved. The efficient conversion of cyclopentene and purine diphenyl is achieved. High selectivity of aldehydes, suitable for industrial production.
Patent Information
- Application Number
- CN202310482468.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-04-28
AI Technical Summary
The existing catalysts have low efficiency, difficulty in recycling and environmental problems in the oxidation of cyclopentene to form glutaraldehyde, and the industrial production costs are high, so they have failed to achieve efficient catalytic effects.
Using a supported phosphotungsten heteropolyacid catalyst, the catalyst is formed by loading quaternary ammonium salts and phosphotungstenic acid on the silica substrate to form an efficient heterogeneous catalyst. The combination of long carbon chain quaternary ammonium salts and phosphotungstenic acid is used to increase the catalyst. The mechanical properties and catalytic activity achieve high efficiency conversion of cyclopentene and high selectivity of glutaraldehyde.
The efficient catalytic effect of cyclopentene conversion rate exceeding 95% and glutaraldehyde selectivity is achieved, which simplifies the separation and recovery of catalysts, has huge industrial application potential, and is simple in the process and is suitable for large-scale production.
Smart Images

Figure CN116474830B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of synthesis technology, and in particular to a synthesis process and an application method for generating high-selective glutaraldehyde by catalyzing cyclopentene oxidation using a supported heteropolyacid quaternary ammonium salt catalyst. Background Art
[0002] The oxidation of cyclopentene to prepare glutaraldehyde is an effective way to transform downstream chemical products into high-value products, replace the traditional pyran process to produce glutaraldehyde, and achieve low-carbon and zero-carbon green industrial development. At present, a variety of catalysts have been used for the one-step oxidation reaction of olefins with hydrogen peroxide, such as zeolites, hydrotalcites, peroxytungsten compounds, polyoxometalates, niobium-based or tungsten-based catalysts, solid acid catalysts, heteropolyacid compound catalysts, etc. It is worth noting that polyoxometalates are transition metal oxygen anion clusters that show high activity in both oxidation reactions and acid-catalyzed reactions. However, the application of polyoxometalate catalysts still has some defects, especially the low efficiency caused by low specific surface area, which causes recovery difficulties and environmental problems.
[0003] Chinese patent CN201410662264.3 discloses a method for preparing a catalyst of a metal-organic framework material UiO-66 doped with a heteropoly acid. The problem with this method is that the preparation process uses a variety of chemical reagents such as phthalic acid and methylformamide, and the catalyst takes a long time to age and roast, resulting in high preparation costs, and is not suitable for an efficient production process for industrial production.
[0004] Chinese patent CN201910646190.7 discloses a tungsten oxide-based mesoporous molecular sieve catalyst, which introduces tungsten oxide as an active component in situ during the preparation of the molecular sieve. The yield of glutaraldehyde in the catalytic oxidation reaction can reach 87%, but the reaction time is controlled to be more than 24 hours, and the effect of efficient catalysis cannot be achieved.
[0005] Chinese patent CN202210888683.3 uses a heteropolyacid ionic liquid solid catalyst. Through the functions of the organic-inorganic parts, the catalyst has good two-phase compatibility and improves the reaction rate. However, the solid catalyst belongs to the ionic liquid catalyst, which has the characteristics of high viscosity and poor mechanical strength. In addition, when used in the liquid phase selective oxidation process, it will be leached by active metals and usually behaves as a homogeneous rather than a heterogeneous catalyst, which brings difficulties to separation and recovery.
[0006] At the above problems, by host-guest interaction, the catalytic activity site is connected to the substrate skeleton, thereby forms discrete and uniform catalytic site on porous system or surface.The quaternary ammonium cation contained on the silicon dioxide substrate simultaneously just provides certain lipophilicity and can transfer peroxy species to the oil phase, has accelerated the contact with substrate in the oil phase, and the three cooperate with each other and can give full play to the advantages of this supported polyacid quaternary ammonium salt catalyst in cyclopentene raw material efficient conversion, glutaraldehyde product high selectivity, simple separation of catalyst.Utilize the advantages of good mechanical property of substrate material, high intensity to combine with heteropolyacid quaternary ammonium salt aspect the cyclopentene efficient catalytic performance among the present invention, realize the effective method of controlling heterogeneous catalytic oxidation reaction degree, have huge actual industrial application potential. Summary of the invention
[0007] To this end, the purpose of the present invention is to combine the advantages of the mechanical properties of mesoporous silica and the efficient catalytic oxidation performance of vacant heteropolyacid quaternary ammonium salts to provide a catalyst with good mechanical properties, high strength and easy separation, and a catalyst for efficient conversion of cyclopentene and high selectivity of glutaraldehyde.
[0008] To this end, the technical solution provided by the present invention is as follows:
[0009] A supported phosphotungstic heteropoly acid catalyst for high-selective synthesis of glutaraldehyde by oxidation of cyclopentene, the supported phosphotungstic heteropoly acid catalyst comprising the following steps in sequence:
[0010] 1) Preparation process of silicon dioxide containing surfactant
[0011] Dissolve a long carbon chain quaternary ammonium salt in a certain amount of deionized water, add 2M NaOH solution and heat to 80°C; add ethyl orthosilicate under stirring, continue the reaction for 2 hours, and a white solid gradually forms in the colorless transparent solution; after the reaction is completed, filter and wash with methanol and deionized water to obtain a white solid, which is silica containing a surfactant.
[0012] 2) Preparation process of silica-supported vacant phosphotungstic heteropoly acid catalyst
[0013] 1) Dissolve phosphotungstic acid in water, add 1M NaHCO3 solution under stirring to adjust the pH of the solution to about 5.0. After stirring at 60°C for 0.5h, add solid sodium chloride and continue stirring for 1h. After the reaction is completed, perform vacuum distillation (-0.1MPa, 55°C) to remove water, recrystallize to obtain a pure solid, and air dry at 70°C to obtain a white solid, which is mono-lacunarity phosphotungstic acid sodium salt Na7PW 11 O 39 .
[0014] 2) Na7PW u O 39The solid was dissolved in water, and a 6M dilute nitric acid solution was added dropwise under stirring to adjust the pH of the solution to about 2.0, and the silicon dioxide described in step 1) was added to the solution according to the mass ratio. Stirring was continued at room temperature for 3 hours, and then filtered and washed with deionized water, and air-dried at 70°C to obtain a white solid as a supported phosphotungstic heteropoly acid catalyst.
[0015] Furthermore, in the above-mentioned supported phosphotungstic heteropolyacid catalyst for the high-selective synthesis of glutaraldehyde by cyclopentene oxidation, the long carbon chain quaternary ammonium salt is a quaternary ammonium salt with an alkyl carbon chain number of 12-18, such as: dodecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium bromide, preferably dodecyltrimethylammonium bromide.
[0016] Furthermore, in the above-mentioned supported phosphotungstic heteropolyacid catalyst for the highly selective synthesis of glutaraldehyde by oxidation of cyclopentene, the mass ratio of the medium-long carbon chain quaternary ammonium salt, deionized water, and tetraethyl orthosilicate in the step 1) is 1:280-290:5.0-6.0.
[0017] Furthermore, in the above-mentioned supported phosphotungstic acid catalyst for the highly selective synthesis of glutaraldehyde by oxidation of cyclopentene, the mass ratio of phosphotungstic acid, deionized water, and sodium chloride solid in the step 2) is 1:10-15:0.10-0.20.
[0018] Further, the above-mentioned supported phosphotungstic heteropoly acid catalyst for the high-selective synthesis of glutaraldehyde by oxidation of cyclopentene, wherein the Na7PW 11 O 39 The mass ratio of the solid to the silicon dioxide solid is 1:0.40-1.50.
[0019] Furthermore, the above-mentioned reaction for the high-selectivity synthesis of glutaraldehyde by oxidation of cyclopentene comprises the following steps: carrying out the reaction in a flask equipped with a magnetic stirrer and a reflux condenser; adding cyclopentene, 30% hydrogen peroxide, a solvent, and a supported catalyst in sequence, and reacting at a certain temperature and time.
[0020] The reaction solvent in the above-mentioned reaction for highly selectively synthesizing glutaraldehyde by oxidation of cyclopentene is selected from one or more of acetonitrile, ethyl acetate, tert-butanol, isopropanol or ethylene dichloride, preferably tert-butanol; the mass ratio of cyclopentene, 30% hydrogen peroxide, solvent tert-butanol, and supported catalyst is: 1:1.25-3.33:1.0-2.0:0.11-0.30, the reaction temperature ranges from 25 to 45°C, and the reaction time is 4 to 8 hours.
[0021] Furthermore, in the above-mentioned reaction for the high-selectivity synthesis of glutaraldehyde by oxidation of cyclopentene, 30% hydrogen peroxide is added in stages, such as a two-stage or three-stage addition method in terms of total reaction time, preferably a two-stage addition method.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. By loading active substances, more active centers are fixed on SiO2, which improves the stability of the catalyst and realizes heterogeneous catalytic reaction, making it easy to recover the catalyst. It is applied to catalytic cyclopentene oxidation reaction. Under mild conditions, the cyclopentene conversion rate reaches more than 95% in a short time, and the glutaraldehyde selectivity is increased to more than 85%.
[0024] 2. Lacunar heteropolyacid salts have great industrial application potential. According to the requirements of the oxidation reaction degree and the reaction environment, the acid strength, homogeneous or heterogeneous phase of the heteropolyacid salts can be designed and optimized in a targeted manner, and the single selective reaction of aldehydes and alcohols can be achieved. In addition, the preparation process of the supported catalyst is simple and can be applied to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is the infrared spectra of supported phosphotungstic heteropoly acid catalysts with different loading amounts;
[0026] Figure 2 is the scanning electron microscope image of the supported phosphotungstic heteropoly acid catalyst with different loading amounts; DETAILED DESCRIPTION
[0027] The present invention is further illustrated by way of examples below, but they do not constitute any limitation to the present invention. Any limited number of modifications made by anyone within the scope of the claims of the present invention are still within the scope of the claims of the present invention.
[0028] Example 1
[0029] Take 5g Na7PW 11 O 39 The solid was dissolved in water, and the pH of the solution was adjusted to about 2.0 with dilute nitric acid solution. 2.00 g of silica solid containing surfactant was added, and the mixture was stirred at room temperature for 3 h, filtered, washed, and air-dried at 70°C to obtain a supported phosphotungstic heteropoly acid catalyst with a loading of 71.4%. Its infrared spectrum can be found at Figure 1 , SEM images see Figure 2 .
[0030] The prepared catalyst was used to catalyze the oxidation reaction of cyclopentene. The reaction was carried out in a flask equipped with a magnetic stirrer, and 50.00 mmol of cyclopentene, 50 mmol of 30% hydrogen peroxide, 8 mL of tert-butyl alcohol, and 0.5 g of a supported catalyst were added in sequence, the reaction temperature was 35°C, and the reaction time was 5 hours. After the reaction was completed, the composition of the components in the reaction mixture was analyzed by gas chromatography, and the catalytic effect was obtained to be 56.88% of cyclopentene conversion rate, 56.89% of glutaraldehyde selectivity, and 29.93% of 1,2-cyclopentanediol selectivity.
[0031] The reaction liquid is directly centrifuged to separate the liquid and the catalyst solid, and the catalyst is washed with ethanol and dried before being reused.
[0032] Example 2
[0033] Take 5g Na7PW 11 O 39 The solid was dissolved in water, and the pH of the solution was adjusted to about 2.0 with dilute nitric acid solution. 2.75 g of silica solid containing surfactant was added, and the mixture was stirred at room temperature for 3 h, filtered, washed, and air-dried at 70°C to obtain a supported phosphotungstic heteropoly acid catalyst with a loading of 64.5%. The infrared spectrum of the catalyst can be found at Figure 1 , SEM images see Figure 2 .
[0034] The prepared catalyst was used to catalyze the oxidation reaction of cyclopentene. The reaction conditions were the same as those in Example 1. After the reaction was completed, the composition of the reaction mixture was analyzed by gas chromatography, and the catalytic effect was 94.82% cyclopentene conversion, 77.06% glutaraldehyde selectivity, and 21.69% 1,2-cyclopentanediol selectivity.
[0035] The reaction liquid is directly centrifuged to separate the liquid and the catalyst solid, and the catalyst is washed with ethanol and dried before being reused.
[0036] Example 3
[0037] Take 5g Na7PW 11 O 39 The solid was dissolved in water, and the pH of the solution was adjusted to about 2.0 with dilute nitric acid solution. 3.75 g of silica solid containing surfactant was added, and the mixture was stirred at room temperature for 3 h, filtered, washed, and air-dried at 70°C to obtain a supported phosphotungstic heteropoly acid catalyst with a loading of 57.1%. Its infrared spectrum can be found at Figure 1 , SEM images see Figure 2 .
[0038] The prepared catalyst was used to catalyze the oxidation reaction of cyclopentene. The reaction conditions were the same as those in Example 1. After the reaction, the components in the reaction mixture were analyzed by gas chromatography, and the catalytic effects were 75.01% cyclopentene conversion, 58.87% glutaraldehyde selectivity, and 25.87% 1,2-cyclopentanediol selectivity.
[0039] The reaction liquid is directly centrifuged to separate the liquid and the catalyst solid, and the catalyst is washed with ethanol and dried before being reused.
[0040] Example 4
[0041] Take 5g Na7PW 11 O 39 The solid was dissolved in water, and the pH of the solution was adjusted to about 2.0 with dilute nitric acid solution. 5.50 g of silica solid containing surfactant was added, and the mixture was stirred at room temperature for 3 h, filtered, washed, and air-dried at 70°C to obtain a supported phosphotungstic heteropoly acid catalyst with a loading of 46.5%. Its infrared spectrum can be found at Figure 1 , SEM images see Figure 2 .
[0042] The prepared catalyst was used to catalyze the oxidation reaction of cyclopentene. The reaction conditions were the same as those in Example 1. After the reaction, the components in the reaction mixture were analyzed by gas chromatography, and the catalytic effects were 68.84% cyclopentene conversion, 35.83% glutaraldehyde selectivity, and 16.18% 1,2-cyclopentanediol selectivity.
[0043] The reaction liquid is directly centrifuged to separate the liquid and the catalyst solid, and the catalyst is washed with ethanol and dried before being reused.
[0044] Example 5
[0045] Take 5g Na7PW 11 O 39 The solid was dissolved in water, and the pH of the solution was adjusted to about 2.0 with dilute nitric acid solution. 2.00 g of silica solid containing surfactant was added, and the mixture was stirred at room temperature for 3 h, filtered, washed, and air-dried at 70°C to obtain a supported phosphotungstic heteropoly acid catalyst with a loading of 64.5%. Its infrared spectrum can be found at Figure 1 , SEM images see Figure 2 .
[0046] The prepared catalyst was used to catalyze the oxidation reaction of cyclopentene. The reaction was carried out in a flask equipped with a magnetic stirrer, and 50.00 mmol of cyclopentene, 50 mmol of 30% hydrogen peroxide, 8 mL of tert-butyl alcohol, and 0.4 g of a supported catalyst were added in sequence, the reaction temperature was 35°C, and the reaction time was 5 hours. After the reaction was completed, the composition of the components in the reaction mixture was analyzed by gas chromatography, and the catalytic effect was obtained to be 89.72% of cyclopentene conversion rate, 52.60% of glutaraldehyde selectivity, and 16.96% of 1,2-cyclopentanediol selectivity.
[0047] The reaction liquid is directly centrifuged to separate the liquid and the catalyst solid, and the catalyst is washed with ethanol and dried before being reused.
[0048] Example 6
[0049] Take 5g Na7PW 11 O 39 The solid was dissolved in water, and the pH of the solution was adjusted to about 2.0 with dilute nitric acid solution. 2.00 g of silica solid containing surfactant was added, and the mixture was stirred at room temperature for 3 h, filtered, washed, and air-dried at 70°C to obtain a supported phosphotungstic heteropoly acid catalyst with a loading of 64.5%. Its infrared spectrum can be found at Figure 1 , SEM images see Figure 2 .
[0050] The prepared catalyst was used to catalyze the oxidation reaction of cyclopentene. The reaction was carried out in a flask equipped with a magnetic stirrer, and 50.00 mmol of cyclopentene, 50 mmol of 30% hydrogen peroxide, 8 mL of tert-butyl alcohol, and 0.6 g of a supported catalyst were added in sequence, the reaction temperature was 35°C, and the reaction time was 5 hours. After the reaction was completed, the composition of the components in the reaction mixture was analyzed by gas chromatography, and the catalytic effect was obtained to be 97.14% of cyclopentene conversion rate, 71.17% of glutaraldehyde selectivity, and 13.57% of 1,2-cyclopentanediol selectivity.
[0051] The reaction liquid is directly centrifuged to separate the liquid and the catalyst solid, and the catalyst is washed with ethanol and dried before being reused.
[0052] Example 7
[0053] Take 5g Na7PW 11 O 39 The solid was dissolved in water, and the pH of the solution was adjusted to about 2.0 with dilute nitric acid solution. 2.00 g of silica solid containing surfactant was added, and the mixture was stirred at room temperature for 3 h, filtered, washed, and air-dried at 70°C to obtain a supported phosphotungstic heteropoly acid catalyst with a loading of 64.5%. Its infrared spectrum can be found at Figure 1 , SEM images see Figure 2 .
[0054] The prepared catalyst was used to catalyze the oxidation reaction of cyclopentene. The reaction was carried out in a flask equipped with a magnetic stirrer, and 50.00mmol of cyclopentene, 50.00mmol of 30% hydrogen peroxide, 8mL of tert-butyl alcohol, and 0.7g of a supported catalyst were added in sequence, the reaction temperature was 35°C, and the reaction time was 5h. After the reaction was completed, the composition of the components in the reaction mixture was analyzed by gas chromatography, and the catalytic effect was obtained to be 96.11% of cyclopentene conversion rate, 63.71% of glutaraldehyde selectivity, and 19.38% of 1,2-cyclopentanediol selectivity.
[0055] The reaction liquid is directly centrifuged to separate the liquid and the catalyst solid, and the catalyst is washed with ethanol and dried before being reused.
[0056] Example 8
[0057] Take 5g Na7PW 11 O 39 The solid was dissolved in water, and the pH of the solution was adjusted to about 2.0 with a dilute nitric acid solution. 2.00 g of silica solid containing a surfactant was added, and the mixture was stirred at room temperature for 3 h, filtered, washed, and air-dried at 70°C to obtain a supported phosphotungstic heteropoly acid catalyst with a loading of 64.5%.
[0058] The prepared catalyst was used to catalyze the oxidation reaction of cyclopentene. The reaction was carried out in a flask equipped with a magnetic stirrer, and 50.00mmol of cyclopentene, 37.50mmol of 30% hydrogen peroxide, 8mL of tert-butyl alcohol, and 0.5g of a supported catalyst were added in sequence, the reaction temperature was 35°C, and the reaction time was 5h. After the reaction was completed, the composition of the components in the reaction mixture was analyzed by gas chromatography, and the catalytic effect was obtained to be 72.58% of cyclopentene conversion rate, 77.75% of glutaraldehyde selectivity, and 19.45% of 1,2-cyclopentanediol selectivity.
[0059] The reaction liquid is directly centrifuged to separate the liquid and the catalyst solid, and the catalyst is washed with ethanol and dried before being reused.
[0060] Example 9
[0061] Take 5g Na7PW 11 O 39 The solid was dissolved in water, and the pH of the solution was adjusted to about 2.0 with a dilute nitric acid solution. 2.00 g of silica solid containing a surfactant was added, and the mixture was stirred at room temperature for 3 h, filtered, washed, and air-dried at 70°C to obtain a supported phosphotungstic heteropoly acid catalyst with a loading of 64.5%.
[0062] The prepared catalyst was used to catalyze the oxidation reaction of cyclopentene. The reaction was carried out in a flask equipped with a magnetic stirrer, and 50.00mmol of cyclopentene, 60.00mmol of 30% hydrogen peroxide, 8mL of tert-butyl alcohol, and 0.5g of a supported catalyst were added in sequence, the reaction temperature was 35°C, and the reaction time was 5h. After the reaction was completed, the composition of the components in the reaction mixture was analyzed by gas chromatography, and the catalytic effect was obtained to be 94.89% of cyclopentene conversion rate, 71.00% of glutaraldehyde selectivity, and 28.12% of 1,2-cyclopentanediol selectivity.
[0063] The reaction liquid is directly centrifuged to separate the liquid and the catalyst solid, and the catalyst is washed with ethanol and dried before being reused.
[0064] Example 10
[0065] Take 5g Na7PW 11 O 39 The solid was dissolved in water, and the pH of the solution was adjusted to about 2.0 with a dilute nitric acid solution. 2.00 g of silica solid containing a surfactant was added, and the mixture was stirred at room temperature for 3 h, filtered, washed, and air-dried at 70°C to obtain a supported phosphotungstic heteropoly acid catalyst with a loading of 64.5%.
[0066] The prepared catalyst was used to catalyze the oxidation reaction of cyclopentene. The reaction was carried out in a flask equipped with a magnetic stirrer, and 50.00mmol of cyclopentene, 100.00mmol of 30% hydrogen peroxide, 8mL of tert-butyl alcohol, and 0.5g of a supported catalyst were added in sequence, the reaction temperature was 35°C, and the reaction time was 5h. After the reaction was completed, the composition of the components in the reaction mixture was analyzed by gas chromatography, and the catalytic effect was obtained to be 87.81% of cyclopentene conversion rate, 63.54% of glutaraldehyde selectivity, and 33.56% of 1,2-cyclopentanediol selectivity.
[0067] The reaction liquid is directly centrifuged to separate the liquid and the catalyst solid, and the catalyst is washed with ethanol and dried before being reused.
[0068] Embodiment 11
[0069] Take 5g Na7PW 11 O 39 The solid was dissolved in water, and the pH of the solution was adjusted to about 2.0 with a dilute nitric acid solution. 2.00 g of silica solid containing a surfactant was added, and the mixture was stirred at room temperature for 3 h, filtered, washed, and air-dried at 70°C to obtain a supported phosphotungstic heteropoly acid catalyst with a loading of 64.5%.
[0070] The prepared catalyst is used to catalyze the oxidation reaction of cyclopentene. The reaction is carried out in a flask equipped with a magnetic stirrer, and 50.00mmol of cyclopentene, 8mL of tert-butyl alcohol, and 0.5g of a supported catalyst are added in sequence. The reaction temperature is 40°C, and the total reaction time is 5h. The two-stage addition of hydrogen peroxide is as follows: 31mmol of 30% hydrogen peroxide is added at 0h of reaction, and 29mmol of 30% hydrogen peroxide is added at 3.5h of reaction. After the reaction is completed, the composition of the components in the reaction mixture is analyzed by gas chromatography, and the catalytic effect is obtained as follows: cyclopentene conversion rate 99.46%, glutaraldehyde selectivity 85.59%, and 1,2-cyclopentanediol selectivity 13.06%.
[0071] The reaction liquid is directly centrifuged to separate the liquid and the catalyst solid, and the catalyst is washed with ethanol and dried before being reused.
[0072] Example 12
[0073] Take 5g Na7PW 11 O 39 The solid was dissolved in water, and the pH of the solution was adjusted to about 2.0 with a dilute nitric acid solution. 2.00 g of silica solid containing a surfactant was added, and the mixture was stirred at room temperature for 3 h, filtered, washed, and air-dried at 70°C to obtain a supported phosphotungstic heteropoly acid catalyst with a loading of 64.5%.
[0074] The prepared catalyst is used to catalyze the oxidation reaction of cyclopentene. The reaction is carried out in a flask equipped with a magnetic stirrer, and 50.00mmol of cyclopentene, 8mL of tert-butyl alcohol, and 0.5g of a supported catalyst are added in sequence. The reaction temperature is 35°C, and the total reaction time is 5h. The three-stage addition of hydrogen peroxide is as follows: 33.5mmol of 30% hydrogen peroxide is added at 0h of reaction, 16.5mmol of 30% hydrogen peroxide is added at 2.5h of reaction, and 10.0mmol of 30% hydrogen peroxide is added at 3.5h of reaction. After the reaction is completed, the composition of the components in the reaction mixture is analyzed by gas chromatography, and the catalytic effect is obtained as follows: cyclopentene conversion rate 94.47%, glutaraldehyde selectivity 84.71%, and 1,2-cyclopentanediol selectivity 13.62%.
[0075] The reaction liquid is directly centrifuged to separate the liquid and the catalyst solid, and the catalyst is washed with ethanol and dried before being reused.
Claims
1. A supported phosphotungstic heteropoly acid catalyst for the highly selective synthesis of glutaraldehyde by cyclopentene oxidation, characterized in that: The supported phosphotungstic heteropoly acid catalyst is prepared by the following steps in sequence: 1) Preparation process of silicon dioxide containing surfactant Dissolve the long carbon chain quaternary ammonium salt in deionized water, add 2M NaOH solution and heat to 80°C; add ethyl orthosilicate under stirring, continue to react for 2 hours, and a white solid gradually forms in the colorless transparent solution; after the reaction is completed, filter and wash with methanol and deionized water to obtain a white solid, which is silica containing a surfactant; 2) Preparation process of silica-supported phosphotungstic heteropoly acid catalyst 1) Dissolve phosphotungstic acid in water, add 1M NaHCO3 solution dropwise while stirring to adjust the solution pH to 5.0; stir at 60°C for 0.5h, then add solid sodium chloride, and continue stirring for 1h; after the reaction is completed, remove water by vacuum distillation, recrystallize to obtain a pure solid, and air dry at 70°C to obtain a white solid, which is mono-lacunarity phosphotungstic heteropoly acid sodium salt Na7PW 11 O 39 ; 2) Na7PW 11 O 39 The solid was dissolved in water, and a 6M dilute nitric acid solution was added dropwise under stirring to adjust the pH of the solution to 2.0, and the silicon dioxide described in step 1) was added to the solution; the stirring was continued at room temperature for 3 hours, and after the stirring was completed, the solution was filtered and washed with deionized water, and air-dried at 70°C to obtain a white solid as a supported phosphotungstic heteropoly acid catalyst; In the step 1), the mass ratio of the medium-long carbon chain quaternary ammonium salt, deionized water, and ethyl orthosilicate is 1:270-300:4.0-7.0; In the step 2), the mass ratio of phosphotungstic acid, water and sodium chloride solid is 1:8-18:0.10-0.20; In step 2) Na7PW 11 O 39 The mass ratio of solid to silica solid is 1:0.30~1.
80.
2. A supported phosphotungstic heteropoly acid catalyst for the high-selective synthesis of glutaraldehyde by cyclopentene oxidation according to claim 1, characterized in that: The long carbon chain quaternary ammonium salt is a quaternary ammonium salt with an alkyl carbon chain number of 12-18.
3. A supported phosphotungstic heteropoly acid catalyst for the high-selective synthesis of glutaraldehyde by cyclopentene oxidation according to claim 2, characterized in that: The quaternary ammonium salt of 12-18 is one of dodecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide, hexadecyltrimethylammonium bromide and octadecyltrimethylammonium bromide.
4. A supported phosphotungstic heteropoly acid catalyst for the highly selective synthesis of glutaraldehyde by cyclopentene oxidation according to claim 1, characterized in that: In the step 1), the mass ratio of the medium-long carbon chain quaternary ammonium salt, deionized water, and ethyl orthosilicate is 1:280-290:5.0-6.
0.
5. A supported phosphotungstic heteropoly acid catalyst for highly selective synthesis of glutaraldehyde by cyclopentene oxidation according to claim 1, characterized in that: In the step 2), the mass ratio of phosphotungstic acid, water and sodium chloride solid is 1:10-15:0.10-0.
20.
6. A supported phosphotungstic heteropoly acid catalyst for highly selective synthesis of glutaraldehyde by cyclopentene oxidation according to claim 1, characterized in that: In step 2) Na7PW 11 O 39 The mass ratio of solid to silica solid is 1:0.40~1.
50.
7. A reaction for synthesizing glutaraldehyde by oxidation of cyclopentene with high selectivity, characterized in that: The reaction is carried out in a flask equipped with a magnetic stirrer and a reflux condenser; cyclopentene, 30% hydrogen peroxide, a solvent, and the supported phosphotungstic heteropoly acid catalyst for high-selective synthesis of glutaraldehyde by oxidation of cyclopentene as claimed in claim 1 are added to the reactor in a mass ratio of 1: 1.25-3.33: 1.0-2.0: 0.11-0.30, and the reaction temperature is 25-45°C, and the reaction time is 4-8 hours; The solvent is one or more of tert-butyl alcohol, acetonitrile, ethyl acetate, isopropanol or ethylene dichloride.