Polyimide and diamine monomer containing quaternary phenyl derivative structure and preparation method thereof
By introducing a tetraphenyl-derived structure and specific side groups into the polyimide film, combined with the polymerization of commercial diamines and dianhydrides, the problem of dielectric constant and loss factor at high frequencies was solved, and low dielectric constant was achieved. , low loss factor and excellent mechanical properties, suitable for high-frequency signal transmission fields.
Patent Information
- Application Number
- CN202310089572.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-06
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-02-06
AI Technical Summary
It is difficult to reduce the dielectric constant and loss factor of existing polyimide films at high frequencies, and their thermal expansion coefficient and water absorption rate are high, making them unable to meet the application needs of high-frequency communications.
Using a polyimide film containing a tetraphenyl-derived structure, a rigid, hydrophobic tetraphenyl main structure is synthesized through a multi-step Suzuki reaction, and hydrogen, fluorine, alkyl and other groups are introduced into the side groups, combined with commercialization Diamine and dianhydride polymerize to control dielectric constant and loss factor.
It achieves the comprehensive performance of high-frequency low dielectric constant, low loss factor, low thermal expansion coefficient, low water absorption, high strength and high modulus, and is suitable for electronic packaging technology fields such as high-frequency signal transmission.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of material science and technology, in particular to the field of high-performance functional polyimide new materials, and relates to a polyimide containing a quaternary phenyl derivative structure, a diamine monomer and a preparation method thereof. Technical Background
[0002] Polyimide films are widely used in flexible printed circuit boards (FCCL) and other fields due to their high strength, excellent insulation performance, dielectric properties, high dimensional stability, high temperature resistance and other advantages. 5G communication uses higher frequency bands for information transmission. Traditional polyimide films such as Kapton (ODA-PMDA) have a higher dielectric constant (D k :3.5,10GHz) and higher loss factor (D f : 0.015,10GHz), resulting in high signal loss and can no longer meet the needs of high-frequency communication.
[0003] Chinese patent CN 109651631B introduces a certain amount of fatty chain structure into the main chain to reduce the loss factor of the polyimide film to 0.003-0.006. However, the introduction of fatty chains will inevitably lead to poor dimensional stability of the PI film, increased thermal expansion coefficient, and poor temperature resistance, making it difficult to apply to FCCL.
[0004] Japanese patent JP2018-80315A proposes the use of a quaternary biphenyl structure to prepare a low-loss polyimide film. However, the dielectric constant of this structure alone is relatively high. The dielectric constant of the system in the patent is 3.47 to 3.57, the loss factor is 0.0027 to 0.0037, and the thermal expansion coefficient is not mentioned, which still cannot meet the application requirements of FCCL.
[0005] Among many structural designs, in order to reduce the dielectric constant of polyimide film, large volume and low polarization structures such as fluorene, triptycene, aliphatic ring, and aliphatic chain are introduced. However, such structures often bring problems such as large high-frequency loss factor and large thermal expansion coefficient. In order to reduce the loss factor, structures such as ester bonds can be introduced, but such structures lead to large dielectric constants. Therefore, how to reduce the dielectric constant of polyimide film while obtaining high-frequency low loss factor, while maintaining its excellent comprehensive performance such as low expansion coefficient, has become a research difficulty in this field.
[0006] In view of this, there is an urgent need in the art for a polyimide film that simultaneously possesses the performance characteristics of high frequency and low dielectric constant, low loss factor, low water absorption, low thermal expansion coefficient, high strength and high modulus. Summary of the invention
[0007] In view of the shortcomings of the prior art, the object of the present invention is to provide a polyimide containing a quaternary derivative structure, which can overcome the problem that the existing polyimide cannot simultaneously achieve high-frequency loss factor, dielectric constant, thermal expansion coefficient, etc.
[0008] Another object of the present invention is to provide a method for preparing the polyimide.
[0009] Another object of the present invention is to provide a diamine monomer containing a quaternary phenyl derivative structure, which can be used as a raw material to synthesize the above-mentioned polyimide.
[0010] Another object of the present invention is to provide a method for preparing a diamine monomer containing a quaternary phenyl derivative structure.
[0011] The technical solution of the present invention is as follows:
[0012] A polyimide containing a quaternary phenyl derivative structure has a repeating structural unit represented by the general formula (I):
[0013]
[0014] Where R A is a tetravalent aromatic hydrocarbon group, R B is a divalent aromatic hydrocarbon group, x and y represent a polymer of repeating structural units, and x:y=100:0-1:99; R1-R8 in the quaterphenyl derivative structure are the same as or different from each other, and are independently selected from hydrogen, fluorine, C1-C10 alkyl, fluorinated C1-C10 alkyl, C1-C10 ester, C1-C10 alkoxy, fluorinated C1-C10 alkoxy, C6-C30 aryl or C6-C30 aryloxy, and at least one of R1-R8 is a non-hydrogen group.
[0015] The preparation method of the polyimide containing a quaternary phenyl derivative structure comprises the following steps: dissolving a diamine monomer containing the quaternary phenyl derivative structure in a solvent, and then adding a solvent containing R A The aromatic dianhydride monomer containing the structure is polymerized to obtain a viscous polyamic acid glue solution, which is then heated and cured after coating to obtain a polyimide film; or the diamine monomer containing the quaternary structure and the diamine monomer containing R B The aromatic diamine monomer of structure is dissolved in a solvent, and then R A Aromatic dianhydride monomers with a structure are polymerized to obtain a viscous polyamic acid adhesive solution, which is then coated and heated to cure to obtain a polyimide film.
[0016] The beneficial effects of the present invention are:
[0017] 1) The present invention adopts a diamine monomer containing a quaternary derivative structure shown in the general formula (II), and obtains a rigid and hydrophobic quaternary main structure by combining a multi-step Suzuki reaction. At the same time, hydrogen, fluorine, C1-C10 alkyl, fluorinated C1-C10 alkyl, C1-C10 ester, C1-C10 alkoxy, fluorinated C1-C10 alkoxy, C6-C30 aryl or C6-C30 aryloxy is introduced at the positions of R1-R8, and at least one of R1-R8 is a non-hydrogen group. The diamine monomer containing a quaternary derivative structure provided by the present invention has a rigid aromatic main chain structure. The polyimide film obtained by polymerizing it with commercial diamine and commercial dianhydride has the advantages of high frequency low loss factor, low thermal expansion coefficient, low water absorption, high strength, high modulus, etc., and while maintaining the high frequency low loss performance, the introduction of R1-R8 groups further reduces the dielectric constant of the PI film.
[0018] 2) The diamine monomer containing a quaternary phenyl derivative structure provided by the present invention further comprises: a , R b , R c , R d , introducing the same or different groups, each independently selected from fluorine, methyl, trifluoromethyl, tert-butyl, oxymethyl or oxybutyl, etc., can further ensure that the polyimide film maintains the advantages of low loss factor, low water absorption, high dimensional stability, high modulus, etc. brought by the quadriphenyl structure. At the same time, low polarity, hydrophobic alkyl groups such as methyl and fluoroalkyl groups such as trifluoromethyl can be introduced through side groups to bring advantages such as low dielectric constant.
[0019] 3) The structure of the polyimide provided by the present invention is shown in the general formula (I). The polyimide film obtained by polymerizing the diamine monomer containing a quaternary derivative structure with commercial diamine and dianhydride has the following excellent comprehensive properties: high frequency and low dielectric constant, low loss factor, low thermal expansion coefficient, low water absorption, high strength, and high modulus. It can be used as a high-performance insulating substrate in the field of electronic packaging technology such as high-frequency signal transmission. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is the H NMR spectrum of the diamine monomer compound of Example 1 of the present invention;
[0021] Figure 2 This is the H NMR spectrum of the diamine monomer compound of Example 2 of the present invention;
[0022] Figure 3 This is the H NMR spectrum of the diamine monomer compound of Example 3 of the present invention;
[0023] Figure 4 This is the H NMR spectrum of the diamine monomer compound of Example 5 of the present invention;
[0024] Figure 5 This is the H NMR spectrum of the diamine monomer compound of Example 6 of the present invention;
[0025] Figure 6 This is the H NMR spectrum of the diamine monomer compound of Example 7 of the present invention;
[0026] Figure 7 This is the H NMR spectrum of the diamine monomer compound of Example 8 of the present invention;
[0027] Figure 8 This is a high-resolution mass spectrum of the diamine monomer compound of Example 5 of the present invention, wherein the upper part is the measured compound signal peak diagram, the lower part is the compound theoretical signal peak diagram, the ordinate Relative Abundance is the relative abundance, and the abscissa m / z is the ratio of the number of protons / the number of charges;
[0028] Fig. 9 This is a high-resolution mass spectrum of the diamine monomer compound of Example 6 of the present invention, wherein the upper part is the measured compound signal peak diagram, the lower part is the compound theoretical signal peak diagram, the ordinate Relative Abundance is the relative abundance, and the abscissa m / z is the ratio of the number of protons / the number of charges;
[0029] Fig.10 This is a mechanical curve diagram of the polyimide film of Application Example 2 of the present invention, wherein the ordinate TensileStrength is the tensile strength, and the abscissa Elongation at break is the elongation at break. A total of five samples were tested, and the average values of the five data are as listed in Table 3;
[0030] Fig.11 This is a mechanical curve diagram of the polyimide film of Application Example 6 of the present invention, wherein the ordinate TensileStrength is the tensile strength, and the abscissa Elongation at break is the elongation at break. A total of five samples were tested, and the average values of the five data are as listed in Table 3. DETAILED DESCRIPTION
[0031] The present invention is a polyimide containing a quaternary phenyl derivative structure, having a repeating structural unit represented by the general formula (I):
[0032]
[0033] Where R A is a tetravalent aromatic hydrocarbon group, R Bis a divalent aromatic hydrocarbon group, x and y represent a polymer of repeating structural units, and x:y=100:0-1:99; R1-R8 in the quaterphenyl derivative structure are the same as or different from each other, and are independently selected from hydrogen, fluorine, C1-C10 alkyl, fluorinated C1-C10 alkyl, C1-C10 ester, C1-C10 alkoxy, fluorinated C1-C10 alkoxy, C6-C30 aryl or C6-C30 aryloxy, and at least one of R1-R8 is a non-hydrogen group.
[0034] Preferably, the C1-C10 alkyl group is selected from methyl, ethyl, propyl, butyl or tert-butyl; the fluorinated C1-C10 alkyl group is selected from trifluoromethyl or pentafluoroethyl; the C6-C30 aryl group is selected from trifluoromethylphenyl or tert-butylphenyl; the C1-C10 ester group is selected from methyl ester, phenyl ester or tert-butylphenyl ester; the C1-C10 alkoxy group is selected from methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy or tert-butoxy; the fluorinated C1-C10 alkoxy group is selected from perfluorobutylethoxy, and the C6-C30 aryloxy group is selected from tert-butylphenoxy or trifluoromethylphenoxy.
[0035] Preferably, x is an integer of 2 to 1000, and y is an integer of 0 to 1000.
[0036] More preferably, the quaternary phenyl derivative structure is selected from the following structures:
[0037]
[0038] Among them, R a , R b , R c , R d are the same as or different from each other, and are each independently selected from fluoro, methyl, trifluoromethyl, tert-butyl, oxymethyl or oxybutyl.
[0039] Most preferably, the quaternary phenyl derivative structure is selected from at least one of the following structures:
[0040]
[0041]
[0042] Preferably, R A At least one selected from the following structures:
[0043] Preferably, R B At least one selected from the following structures:
[0044]
[0045] The preparation method of the polyimide containing a quaternary phenyl derivative structure comprises the following steps: dissolving a diamine monomer containing the quaternary phenyl derivative structure in a solvent, and then adding a A The aromatic dianhydride monomer containing the structure is polymerized to obtain a viscous polyamic acid glue solution, which is then heated and cured after coating to obtain a polyimide film; or the diamine monomer containing the quaternary phenyl derivative structure and the diamine monomer containing R B The aromatic diamine monomer of structure is dissolved in a solvent, and then R A Aromatic dianhydride monomers with a structure are polymerized to obtain a viscous polyamic acid adhesive solution, which is then coated and heated to cure to obtain a polyimide film.
[0046] Preferably, the diamine monomer containing a quaternary phenyl derivative structure is a structure represented by the general formula (II):
[0047]
[0048] Among them, R1~R8 are the same as or different from each other, and are independently selected from hydrogen, fluorine, C1~C10 alkyl, fluorinated C1~C10 alkyl, C1~C10 ester, C1~C10 alkoxy, fluorinated C1~C10 alkoxy, C6~C30 aryl or C6~C30 aryloxy, and at least one of R1~R8 is a non-hydrogen group.
[0049] The said R A The aromatic dianhydride monomer of the structure can be a commercially available product, preferably at least one of the following aromatic dianhydride monomers: 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 4,4'-oxydiphthalic anhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxylic acid)hexafluoropropane dianhydride, 4,4'-phenylenedioxydiphthalic anhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 3,3',4,4'-diphenyl sulfonetetracarboxylic dianhydride, 4,4'-(4,4'-isopropyldiphenyloxy)phthalic anhydride, p-phenylene-diphenyltrimethylol dianhydride;
[0050] Contains R BThe aromatic diamine monomer of the structure can be a commercially available product, preferably at least one of the following aromatic diamine monomers: p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 4,4"-diaminoquaterphenyl, 4,4"-diaminoterphenyl, 1,3-bis(4'-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 2,2'-bis(trifluoromethyl)-4,4'-diaminobenzene ether, 2,2'-difluoro-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)diaminobiphenyl, 4,4'-diamino-2,2'-dimethyl-1,1'-biphenyl, 2,2'-bis[4-(4-aminophenoxyphenyl)]propane, 4,4'-diaminobenzoic acid phenyl ester, di-p-aminophenyl terephthalate, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminobiphenyl, 2 2'-Diaminodiphenyl sulfide, 4,4-diaminodiphenyl sulfide, 4,4'-bis(3-aminophenoxy)benzophenone, 3,3',5,5'-tetramethylbenzidine, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)diphenyl sulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane.
[0051] The diamine monomer containing a quaternary phenyl derivative structure comprises R B Aromatic diamine monomers having the structure R A The addition ratio of the aromatic dianhydride monomer containing the structure can adjust the performance of the PI film. Preferably, the diamine monomer containing the quaternary phenyl derivative structure and the diamine monomer containing R B The molar ratio of the aromatic diamine monomer of the structure is 10% to 100%: 0 to 90%, and more preferably 50% to 100%: 0 to 50%. A The total molar ratio of the aromatic dianhydride monomer of the structure to the aforementioned diamine monomer is 0.99 to 1.01, more preferably 0.995 to 1.005. The components of the dianhydride monomer can be combined and adjusted according to performance requirements.
[0052] Preferably, the solvent is at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide and γ-butyrolactone; the viscous polyamic acid glue has a solid content of 5wt% to 30wt% and a viscosity of 10000 to 200000 mPa·S; the coated substrate can be a glass plate or a metal carrier; the heating curing method is an inert gas atmosphere, a heating rate of 1 to 5°C / min, a maximum temperature of 300 to 500°C, and a constant temperature time of 10 to 60min. More preferably, the heating rate is 2 to 3°C / min, the maximum temperature is 350 to 400°C, and the constant temperature time is 20 to 30min.
[0053] The present invention provides a diamine monomer containing a quaternary phenyl derivative structure, which has the structure shown below:
[0054]
[0055]
[0056] The present invention provides a method for preparing a diamine monomer containing a quaternary phenyl derivative structure, comprising the following sequential steps: (1) preparing a compound A2 by Miyaura borate esterification reaction of a raw material A1;
[0057] (2) A2 and an excess of halide A3 undergo Suzuki coupling reaction to prepare a new halide A4;
[0058] (3) A4 is subjected to Suzuki reaction with phenylboronic acid or boric acid ester A5 having an amino group or a nitro group to prepare compound A6;
[0059] (4) A6 is subjected to Suzuki reaction with phenylboronic acid or boric acid ester A7 having an amino group or a nitro group to prepare compound A8; (5) A8 is reduced to obtain the target product of the general formula (II);
[0060] The synthesis path is as follows:
[0061]
[0062] Wherein, X is a halogen; Y is a borate or boric acid; Z1 and Z2 are amino or nitro groups; when compound A4 is commercially available, steps (1) and (2) are omitted; when A5 is the same as A7, steps (3) and (4) are combined into one step; when Z1 and Z2 are amino groups, step (5) is omitted, and A8 is the target product of general formula (II); when Z1 or Z2 carries a nitro group, A8 is reduced by step (5) to obtain the target product of general formula (II); wherein R1 to R8 are the same or different and are independently selected from hydrogen, fluorine, C1 to C10 alkyl, fluorinated C1 to C10 alkyl, C1 to C10 ester, C1 to C10 alkoxy, fluorinated C1 to C10 alkoxy, C6 to C30 aryl or C6 to C30 aryloxy, and at least one of R1 to R8 is a non-hydrogen group.
[0063] Preferably, in step (1), under the protection of an inert gas, compound A1 is added to a solvent, and then diboric acid pinacol ester, a base, and a palladium catalyst are added. After the reaction, the solvent is removed, and compound A2 is obtained by separation and purification.
[0064] In step (2), under the protection of inert gas, compound A2 is added to a solvent, a catalytic amount of a catalyst is added, an alkali solution is added, and then compound A3 is added to react. After the reaction is completed, the liquids are separated, the solvent is removed by rotary evaporation, and compound A4 is obtained after separation and purification;
[0065] In steps (3) and (4), under the protection of inert gas, raw materials are added to the solvent, a catalytic amount of catalyst is added, an alkali solution is added, and then a compound with an amino group or a nitro group is added to react. After the reaction is completed, the liquids are separated, the solvent is removed by rotary evaporation, and the corresponding product is obtained after separation and purification;
[0066] In step (5), after removing the air, the raw materials are added and the target product of general formula (II) is prepared by reduction reaction.
[0067] Preferably, in step (1), the solvent is one of dimethyl sulfoxide, DMF, dioxane, and toluene, the palladium catalyst is one of [1,1'-bis(diphenylphosphino)ferrocene]dichloropalladium, [1,1'-bis(diphenylphosphino)ferrocene]dichloropalladium dichloromethane complex, and the base is potassium carbonate, potassium phosphate or potassium acetate, more preferably potassium acetate. Preferably, the reaction temperature is 80 to 110°C, more preferably 90 to 100°C.
[0068] Preferably, in steps (2), (3) and (4), the solvent is at least one of tetrahydrofuran, dioxane, toluene, ethanol and DMF, the catalyst is one of tetrakistriphenylphosphine palladium and triphenylphosphine / palladium acetate, and the base is one of sodium carbonate, potassium carbonate, potassium phosphate, cesium fluoride, cesium carbonate, barium hydroxide and sodium hydroxide; preferably, the reaction temperature is 65 to 100°C, more preferably 70 to 80°C.
[0069] Preferably, in step (5), the reduction reaction may be a hydrogen reduction reaction under Pd / C catalysis, a reduction reaction under Fe / dilute hydrochloric acid, a reduction reaction under stannous chloride / dilute hydrochloric acid, or a hydrazine hydrate reduction reaction under Pd / C catalysis.
[0070] The following examples are provided for a better understanding of the present invention, but are not limited to the best mode of implementation, and do not limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0071] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0072] Example 1
[0073] This embodiment provides a diamine monomer containing a quaternary phenyl derivative structure, and the synthesis path of the compound is as follows:
[0074]
[0075] The preparation method of the compound is specifically as follows:
[0076] (1) 2.5-dibromo-1.4-dimethoxybenzene (5.92 g, 20 mmol), 100 mL of dioxane, bipyraclostrobin (5.08 g, 20 mmol), potassium acetate (2.94 g 30 mmol), and a catalytic amount of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride were added to a 250 mL two-necked flask. The mixture was kept under argon atmosphere and reacted at 100° C. for 24 h. After the reaction was completed, the solvent was removed by filtration and rotary evaporation. After purification by column chromatography, a white solid A was obtained.
[0077] (6.17 g, 90%).
[0078] (2) In a 250 mL double-necked flask, intermediate A (6.17 g, 18 mmol), tetrahydrofuran (150 mL), p-dibromobenzene (8.50 g, 36 mmol), potassium carbonate aqueous solution (2 M, 27 mL), and a catalytic amount of tetrakistriphenylphosphine palladium were added. The mixture was kept under argon atmosphere and reacted at 80° C. for 24 h. After the reaction was completed, the liquid was separated and the solvent was removed by rotary evaporation. After purification by column chromatography, a white solid B (5.62 g, 84%) was obtained.
[0079] (3) Add intermediate B (5.58 g, 15 mmol), tetrahydrofuran 100 mL, p-aminophenylboronic acid (6.16 g, 45 mmol), potassium carbonate aqueous solution (2 M, 45 mL), and catalytic amount of tetrakistriphenylphosphine palladium to a 250 mL two-necked flask, and react at 80°C for 24 h. After the reaction is completed, separate the liquids, remove the solvent by rotary evaporation, and purify by column chromatography to obtain a beige solid, which is the target compound (4.40 g, 74%). The H NMR spectrum of the compound is as follows Figure 1 As shown, high resolution mass spectrometry HRMS m / z: [m+H] + Calculate for C 26 H 24 N2O2,397.19105, found 397.19095
[0080] Example 2
[0081]
[0082] The same preparation steps as in Example 1 were used, except that the raw material was replaced with 1,4-dibromo-tetramethylbenzene instead of 2.5-dibromo-1,4-dimethoxybenzene, and the target compound was finally prepared as a white solid. Figure 2 As shown, high resolution mass spectrometry HRMS m / z: [m+H] + Calculate for C 28H 28 N2,393.23253, found 393.23239
[0083] Example 3
[0084]
[0085] The same experimental steps as in Example 1 were used to prepare the compound by replacing the raw material from 2.5-dibromo-1.4-dimethoxybenzene with 2.5-dibromo-1-trifluoromethylbenzene. The H NMR spectrum of the compound is shown in Figure 3 As shown, high resolution mass spectrometry HRMS m / z: [m+H] + Calculate for C 25 H 19 F3N2,405.15731,found 405.15759.
[0086] Example 4
[0087]
[0088] The same as Example 3, the raw materials were changed to prepare the compound, high resolution mass spectrum HRMS m / z: [m+H] + calcdfor C 25 H 22 N2,351.18121,found 351.18144.
[0089] Example 5
[0090]
[0091] The same experimental steps as in Example 1 were used to prepare the compound by replacing the raw material with 2.5-dibromo-1.4-dimethoxybenzene. The H NMR spectrum of the compound is shown in Figure 5 As shown, high resolution mass spectrometry HRMS m / z: [m+H] + Calculate for C 26 H 24 N2,365.20123,found365.20132.
[0092] Example 6
[0093]
[0094] The same experimental steps as in Example 1 were used to prepare the compound by replacing the raw material from 2.5-dibromo-1.4-dimethoxybenzene with 1,4-dibromo-2,5-bistrifluoromethylbenzene. The H NMR spectrum of the compound is shown in Figure 6As shown, high resolution mass spectrometry HRMS m / z: [m+H] + Calculate for C 26 H 18 F6N2,473.14469, found 473.14438.
[0095] Example 7
[0096]
[0097] The preparation route is as shown above, with the same experimental steps as in Example 1, except that the raw material is replaced by 2.5-dibromo-1.4-dimethoxybenzene with 2.5-dibromo-1.4-dimethylbenzene; in the second step, the raw material is replaced by 1,4-dibromobenzene with 2.5-dibromo-1.4-dimethylbenzene to prepare the compound. The NMR spectrum of the compound is shown in Figure 7 As shown, high resolution mass spectrometry HRMS m / z: [m+H] + Calculate for C 28 H 28 N2,393.23253, found 393.23215.
[0098] Example 8
[0099]
[0100] The same method as in Example 7 was used, except that 2.5-dibromo-1.4-dimethylbenzene was replaced with 2.5-dibromo-1.4-difluorobenzene to prepare the compound. Figure 8 As shown, high resolution mass spectrometry HRMS m / z: [m+H] + Calculate for C 24 H 16 F4N2,409.13224,found 409.13141.
[0101] Example 9
[0102]
[0103] The same as Example 7, the raw materials were changed to synthesize the compound, high resolution mass spectrum HRMS m / z: [m+H] + Calculate for C 26 H 24 N2,365.20123, found 365.20131.
[0104] Example 10
[0105]
[0106] Same as Example 2, the raw materials were changed to synthesize the compound, high resolution mass spectrometry HRMS m / z: [m+H] + Calculate for C 24 H 16 F4N2,409.13224,found 409.13261.
[0107] Embodiment 11
[0108]
[0109] Same as Example 7, the raw materials were changed to synthesize the compound, high resolution mass spectrum HRMS m / z: [m+H] + Calculate for C 28 H 16 F 12 N2,609.11212,found 609.11235.
[0110] Example 12
[0111]
[0112] Same as Example 1, the raw materials were changed to synthesize the compound, high resolution mass spectrometry HRMS m / z: [m+H] + Calculate for C 32 H 36 N2,448.29930,found 448.29920.
[0113] Example 13
[0114]
[0115] Same as Example 1, the raw materials were changed to synthesize the compound, high resolution mass spectrometry HRMS m / z: [m+H] + Calculate for C 32 H 36 N2O2,481.48226, found 481.48245.
[0116] Application Example 1
[0117] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0118] (1) Under nitrogen protection, the diamine monomer compound (1.0514 g, 3 mmol) obtained in Example 4 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (17.40 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (0.8827 g, 3 mmol) was added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0119] (2) After vacuum defoaming, the polyamic acid glue solution was coated on a clean glass plate and heated to cure in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 360°C at 2°C / min, and the temperature was maintained at 360°C for 30 min.
[0120] The repeating structural unit of the polyimide film is as follows:
[0121]
[0122] Application Example 2
[0123] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0124] (1) Under nitrogen protection, the diamine monomer compound (1.1895 g, 3 mmol) obtained in Example 1 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (18.65 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (0.8827 g, 3 mmol) was added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0125] (2) After vacuum defoaming, the polyamic acid glue solution was coated on a clean glass plate and heated to cure in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 360°C at 2°C / min, and the temperature was maintained at 360°C for 30 min.
[0126] The repeating structural unit of the polyimide film is as follows:
[0127]
[0128] Application Example 3
[0129] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0130] (1) Under nitrogen protection, the diamine monomer compound (1.1776 g, 3 mmol) obtained in Example 2 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (18.54 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (0.8827 g, 3 mmol) was added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0131] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0132] The repeating structural unit of the polyimide film is as follows:
[0133]
[0134] Application Example 4
[0135] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0136] (1) Under nitrogen protection, the diamine monomer compound (1.2133 g, 3 mmol) obtained in Example 3 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (18.86 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (0.8827 g, 3 mmol) was added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0137] (2) After vacuum defoaming, the polyamic acid glue solution was coated on a clean glass plate and heated to cure in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 360°C at 2°C / min, and the temperature was maintained at 360°C for 30 min.
[0138] The repeating structural unit of the polyimide film is as follows:
[0139]
[0140] Application Example 5
[0141] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0142] (1) Under nitrogen protection, the diamine monomer compound (1.0935 g, 3 mmol) obtained in Example 9 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (17.78 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (0.8827 g, 3 mmol) was added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0143] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0144] The repeating structural unit of the polyimide film is as follows:
[0145]
[0146] Application Example 6
[0147] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0148] (1) Under nitrogen protection, the diamine monomer compound (1.0935 g, 3 mmol) obtained in Example 5 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (17.78 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (0.8827 g, 3 mmol) was added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0149] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0150] The repeating structural unit of the polyimide film is as follows:
[0151]
[0152] Application Example 7
[0153] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0154] (1) Under nitrogen protection, the diamine monomer compound (1.1776 g, 3 mmol) obtained in Example 7 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (18.54 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (0.8827 g, 3 mmol) was added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0155] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0156] The repeating structural unit of the polyimide film is as follows:
[0157]
[0158] Application Example 8
[0159] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0160] (1) Under nitrogen protection, the diamine monomer compound (1.3460 g, 3 mmol) obtained in Example 12 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (14.91 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (0.8827 g, 3 mmol) was added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0161] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0162] The repeating structural unit of the polyimide film is as follows:
[0163]
[0164] Application Example 9
[0165] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0166] (1) Under nitrogen protection, the diamine monomer compound (1.4173 g, 3 mmol) obtained in Example 6 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (15.39 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (0.8827 g, 3 mmol) was added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0167] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0168] The repeating structural unit of the polyimide film is as follows:
[0169]
[0170] Application Example 10
[0171] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0172] (1) Under nitrogen protection, the diamine monomer compound (1.2252 g, 3 mmol) obtained in Example 8 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (14.11 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (0.8827 g, 3 mmol) was added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0173] (2) After vacuum defoaming, the polyamic acid glue solution was coated on a clean glass plate and heated to cure in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 360°C at 2°C / min, and the temperature was maintained at 360°C for 30 min.
[0174] The repeating structural unit of the polyimide film is as follows:
[0175]
[0176] Application Example 11
[0177] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0178] (1) Under nitrogen protection, the diamine monomer compound (1.4420 g, 3 mmol) obtained in Example 13 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (13.17 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (0.8827 g, 3 mmol) was added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0179] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 300°C at 2°C / min, and the temperature was kept at 300°C for 30 min.
[0180] The repeating structural unit of the polyimide film is as follows:
[0181]
[0182] Application Example 12
[0183] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0184] (1) Under nitrogen protection, the diamine monomer compound (0.8089 g, 2 mmol) obtained in Example 3 and 2,2'-bis(trifluoromethyl)diaminobiphenyl TFMB (0.6405, 2 mmol) were accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (11.96 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (1.1769 g, 4 mmol) was added, and the reaction was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0185] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0186] The repeating structural unit of the polyimide film is as follows:
[0187]
[0188] Application Example 13
[0189] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0190] (1) Under nitrogen protection, the diamine monomer compound (0.7280 g, 1.8 mmol) obtained in Example 3 and 2,2'-bis(trifluoromethyl)diaminobiphenyl TFMB (1.3450 g, 4.2 mmol) were accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (15.35 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (1.7653 g, 6 mmol) was added, and the reaction was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0191] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0192] The repeating structural unit of the polyimide film is as follows:
[0193]
[0194] Application Example 14
[0195] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0196] (1) Under nitrogen protection, the diamine monomer compound (0.7851 g, 2 mmol) and 2,2'-bis(trifluoromethyl)diaminobiphenyl TFMB (0.6405 g, 2 mmol) prepared in Example 2 were accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (14.74 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (1.1769 g, 4 mmol) was added, and the reaction was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0197] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0198] The repeating structural unit of the polyimide film is as follows:
[0199]
[0200] Application Example 15
[0201] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0202] (1) Under nitrogen protection, the diamine monomer compound (1.5702 g, 4 mmol) prepared in Example 2 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (13.34 g) was added, and after stirring to dissolve, 4,4'-(4,4'-isopropyldiphenyloxy)bis(phthalic anhydride) BPADA (0.4164 g, 0.8 mmol) and 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (0.9415 g, 3.2 mmol) were added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0203] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0204] The repeating structural unit of the polyimide film is as follows:
[0205]
[0206] Application Example 16
[0207] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0208] (1) Under nitrogen protection, the diamine monomer compound (0.8748 g, 2.4 mmol) and 2,2'-bis[4-(4-aminophenoxyphenyl)]propane BAPP (0.2463 g, 0.6 mmol) prepared in Example 9 were accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (12.82 g) was added, and 3,3',4,4'-benzophenonetetracarboxylic dianhydride BTDA (0.9667 g, 3.0 mmol) was added after stirring to dissolve. The mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0209] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0210] The repeating structural unit of the polyimide film is as follows:
[0211]
[0212] Application Example 17
[0213] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0214] (1) Under nitrogen protection, the diamine monomer compound (1.0935 g, 3.0 mmol) obtained in Example 5 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (18.21 g) was added, and after stirring to dissolve, 4,4'-oxydiphthalic anhydride ODPA (0.9306 g, 3.0 mmol) was added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0215] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0216] The repeating structural unit of the polyimide film is as follows:
[0217]
[0218] Application Example 18
[0219] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0220] (1) Under nitrogen protection, the diamine monomer compound (1.4173 g, 3.0 mmol) obtained in Example 6 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (14.68 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (0.7061 g, 2.4 mmol) and 4,4'-(hexafluoroisopropylene) diphthalic anhydride 6FDA (0.2665 g, 0.6 mmol) were added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0221] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0222] The repeating structural unit of the polyimide film is as follows:
[0223]
[0224] Application Example 19
[0225] This embodiment provides a polyimide film, and the preparation method thereof comprises the following steps:
[0226] (1) Under nitrogen protection, the diamine monomer compound (1.4420 g, 3 mmol) obtained in Example 13 was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (17.20 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride BPDA (0.4413 g, 1.5 mmol) and p-phenylene-diphenyltrimethylol dianhydride TAHQ (0.6875 g, 1.5 mmol) were added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0227] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 300°C at 2°C / min, and the temperature was kept at 300°C for 30 min.
[0228] The repeating structural unit of the polyimide film is as follows:
[0229]
[0230] Comparative Example 1
[0231] This comparative example provides a polyimide film, and the preparation method thereof comprises the following steps:
[0232] (1) Under nitrogen protection, accurately weigh the diamine monomer 4,4'-diaminodiphenyl ether ODA (1.2014 g, 6 mmol) in a 30 mL round-bottom flask, add anhydrous DMAc (14.22 g), stir to dissolve, then add pyromellitic anhydride PMDA (1.3087 g, 6 mmol), stir to react for 24 h, and obtain a viscous polyamic acid glue solution.
[0233] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 400°C at 2°C / min, and the temperature was kept at 400°C for 30 min.
[0234] The repeating structural unit of the polyimide film is as follows:
[0235]
[0236] Comparative Example 2
[0237] This comparative example provides a polyimide film, and the preparation method thereof comprises the following steps:
[0238] (1) Under nitrogen protection, p-phenylenediamine (0.7570 g, 7 mmol) was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (15.96 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (2.0595 g, 7 mmol) was added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0239] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 400°C at 2°C / min, and the temperature was kept at 400°C for 30 min.
[0240] The repeating structural unit of the polyimide film is as follows:
[0241]
[0242] Comparative Example 3
[0243] This comparative example provides a polyimide film, and the preparation method thereof comprises the following steps:
[0244] (1) Under nitrogen protection, accurately weigh the diamine monomer 2,2'-bis(trifluoromethyl)diaminobiphenyl TFMB (1.6011 g, 5 mmol) in a 30 mL round-bottom flask, add anhydrous DMAc (14.00 g), stir to dissolve, then add 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (1.4711 g, 5 mmol), stir to react for 24 h, and obtain a viscous polyamic acid glue solution.
[0245] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0246] The repeating structural unit of the polyimide film is as follows:
[0247]
[0248] Comparative Example 4
[0249] This comparative example provides a polyimide film, and the preparation method thereof comprises the following steps:
[0250] (1) Under nitrogen protection, diamine monomer 4,4'-diamino-2,2'-dimethyl-1,1'-biphenyl (1.0614 g, 5 mmol) was accurately weighed in a 30 mL round-bottom flask, anhydrous DMAc (14.35 g) was added, and after stirring to dissolve, 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (1.4711 g, 5 mmol) was added, and the mixture was stirred for 24 h to obtain a viscous polyamic acid glue solution.
[0251] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 350°C at 2°C / min, and the temperature was maintained at 350°C for 30 min.
[0252] The repeating structural unit of the polyimide film is as follows:
[0253]
[0254] Comparative Example 5
[0255] This comparative example provides a polyimide film, and the preparation method thereof comprises the following steps:
[0256] (1) Under nitrogen protection, accurately weigh the diamine monomer 4,4"-diaminoquaternaryl (1.009 g, 3 mmol) in a 30 mL round-bottom flask, add anhydrous DMAc (17.03 g), stir to dissolve, then add 3,3',4,4'-biphenyltetracarboxylic dianhydride BPDA (0.8827 g, 3 mmol), stir to react for 24 h, and obtain a viscous polyamic acid glue solution.
[0257] (2) The polyamic acid glue solution was vacuum defoamed and then coated on a clean glass plate. It was then heated and cured in a nitrogen atmosphere. The curing procedure was 80°C for 1 h, then the temperature was increased to 400°C at 2°C / min, and the temperature was kept at 400°C for 30 min.
[0258] The repeating structural unit of the polyimide film is as follows:
[0259]
[0260] Test Results
[0261] The H NMR spectrum of the monomer was obtained by Bruker's AVANCE III 400 NMR spectrometer. The solvent used in the test was deuterated dimethyl sulfoxide (DMSO-d6) or deuterated chloroform (CDCl3), and the concentration of the sample during the H NMR test was about 4 mg mL -1 .
[0262] The high-resolution mass spectrometry test of the monomer was obtained by the German Thermo Fisher high-resolution orbital trap liquid-mass spectrometer Q Exactive hydrogenation test.
[0263] The test method for the high-frequency dielectric constant and loss factor of polyimide film is as follows: the vector network analyzer P5003A of Keysight Technologies is used, the resonant cavity is the separated column dielectric resonant cavity (10GHz) of QWED of Poland, the environmental humidity is controlled at 50% RH, and the temperature is 25°C.
[0264] The test method of water absorption rate is as follows: the film is vacuum dried at 150℃ for 12 hours, then transferred to a dryer and restored to room temperature, and then weighed to obtain W0. The film is placed in water and soaked at 25℃ for 12 hours, then taken out and the surface water is wiped clean, and then weighed W1. The water absorption rate is: (W1-W0) / W0*100%.
[0265] Test method for mechanical properties (tensile strength, elongation at break, elastic modulus): obtained by tensile machine test according to national standard GB / T 1040.1-2018, five specimens are tested for each application embodiment, and the average of the five values is the final result, as listed in Table 3.
[0266] Thermal expansion coefficient test of polyimide film: Use TA company D450 equipment, heat up to 200℃ at 10℃ / min, then cool down to 50℃ at 10℃ / min, and then heat up to 400℃ at 10℃ / min. The linear expansion coefficient CTE takes the temperature range of 100-200℃.
[0267] The composition of the quaternary phenyl-containing high-frequency low-loss polyimide film is shown in the following Table 1. Mole % represents the molar ratio of each monomer in the total diamine and dianhydride.
[0268] The polyimide films prepared in the application examples and comparative examples were tested according to the above method, and the obtained data are shown in Table 2 and Table 3.
[0269] Table 1 Monomer composition and ratio of the series of polyimide films listed in this patent
[0270]
[0271] Table 2. Parameter comparison of polyimide films prepared in the application examples and comparative examples
[0272]
[0273]
[0274] Table 3 Mechanical properties of films
[0275] Tensile strength(MPa) Elastic film quantity (GPa) Elongation at break (%) Application Example 1 415 8.6 38.5 Application Example 2 434 8.8 35.2 Application Example 3 330 6.9 39.3 Application Example 4 403 7.6 42.3 Application Example 5 421 8.1 41.2 Application Example 6 435 8.4 39.0 Application Example 7 414 8.0 24.1 Application Example 8 350 7.2 27.0 Application Example 9 385 7.2 40.3 Application Example 10 310 7.8 20.1 Application Example 11 320 6.4 35.6 Application Example 12 372 6.7 39.4 Application Example 13 303 6.5 22.5 Application Example 14 381 6.9 38.6 Application Example 15 210 5.2 51.7 Application Example 16 250 5.5 40.6 Application Example 17 315 6.8 36.7 Application Example 18 290 5.7 32.2 Application Example 19 308 6.3 26.2 Comparative Example 1 160 2.2 35.6 Comparative Example 2 305 7.5 20.1 Comparative Example 3 195 5.5 10.4 Comparative Example 4 300 7.9 10.0 Comparative Example 5 255 7.5 17.2
[0276] The above examples clearly illustrate the advantages of the diamine monomer structure containing a quaternary derivative structure designed by the present invention in high-frequency and low-loss polyimide films: while having a sufficiently low loss factor, by introducing groups such as methyl, trifluoromethyl, fluorine atoms, and tert-butyl groups, the dielectric constant of the polyimide film is effectively reduced, and excellent comprehensive performance is obtained: it has very low water absorption, a low thermal expansion coefficient, and excellent mechanical properties. The specific data analysis is as follows:
[0277] The loss factors of common polyimide films such as ODA-PMDA and PPD-BPDA in the comparative examples are as high as 0.00568 to 0.0130, while the loss factors in the embodiments are 0.00248 to 0.00581, most of which are lower than 0.0035. The loss factors are generally low, which meets the use requirements of low loss factors in the field of high-frequency communications; for example, although the polyimide film polymerized by pure tetraphenyl diamine monomer and BPDA can have a low loss factor of 0.00262, its dielectric constant is as high as 3.71, which cannot meet the low dielectric constant requirements in the field of high-frequency communications. On this basis, by introducing methyl, trifluoromethyl, fluorine atom, tert-butyl and other groups, the dielectric constant is reduced from 3.71 to 3.05 to 3.60, most of which are lower than 3.35. At the same time, the mechanical properties of the embodiment include tensile strength of 210-435 MPa, modulus of 5.2-8.8 Gpa, elongation at break of 24.1%-51.7%, coefficient of thermal expansion CTE of -3.7-22.5, and water absorption of less than 0.9%. It has excellent comprehensive performance and is particularly suitable as a high-performance insulating substrate for use in electronic packaging technology fields such as high-frequency signal transmission.
Claims
1. A polyimide containing a quaternary phenyl derivative structure, having a repeating structural unit represented by the general formula (I): in is a tetravalent aromatic hydrocarbon group, R B is a divalent aromatic hydrocarbon group, x and y represent the degree of polymerization of the repeating structural unit, x:y = 100:0 to 1:99; quaternary derivative structure R1~R8 are the same as or different from each other, and are independently selected from hydrogen, fluorine, C1~C10 alkyl, fluorinated C1~C10 alkyl, C1~C10 ester, C1~C10 alkoxy, fluorinated C1~C10 alkoxy, C6~C30 aryl or C6~C30 aryloxy, and at least one of R1~R8 is a non-hydrogen group.
2. The polyimide containing a quaternary phenyl derivative structure according to claim 1, characterized in that: The C1-C10 alkyl group is selected from methyl, ethyl, propyl, and butyl; the fluorinated C1-C10 alkyl group is selected from trifluoromethyl or pentafluoroethyl; the C6-C30 aryl group is selected from trifluoromethylphenyl or tert-butylphenyl; the C1-C10 ester group is selected from methyl ester, phenyl ester or tert-butylphenyl ester; the C1-C10 alkoxy group is selected from methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy or tert-butoxy; the fluorinated C1-C10 alkoxy group is selected from perfluorobutylethoxy, and the C6-C30 aryloxy group is selected from tert-butylphenoxy or trifluoromethylphenoxy.
3. The polyimide containing a quaternary phenyl derivative structure according to claim 1, characterized in that: The quaternary phenyl derivative structure is selected from at least one of the following structures: Among them, R a , R b , R c , R d are the same as or different from each other, and are each independently selected from fluoro, methyl, trifluoromethyl, tert-butyl, oxymethyl or oxybutyl.
4. The polyimide containing a quaternary phenyl derivative structure according to claim 1, characterized in that: The quaternary phenyl derivative structure is selected from at least one of the following structures:
5. The polyimide containing a quaternary phenyl derivative structure according to claim 4, characterized in that: The At least one selected from the following structures:
6. The polyimide containing a quaternary phenyl derivative structure according to claim 4, characterized in that: The R B At least one selected from the following structures:
7. The method for preparing the polyimide containing a quaternary phenyl derivative structure according to claim 1, comprising the steps of: dissolving a diamine monomer containing the quaternary phenyl derivative structure in a solvent, and then adding The aromatic dianhydride monomer containing the structure is polymerized to obtain a viscous polyamic acid glue solution, which is then heated and cured after coating to obtain a polyimide film; or the diamine monomer containing the quaternary phenyl derivative structure and the diamine monomer containing R B The aromatic diamine monomer of structure is dissolved in a solvent, and then added Aromatic dianhydride monomers with a structure are polymerized to obtain a viscous polyamic acid adhesive solution, which is then coated and heated to cure to obtain a polyimide film.
8. The method for preparing a polyimide containing a quaternary phenyl derivative structure according to claim 7, characterized in that: The diamine monomer containing a quaternary phenyl derivative structure is a structure shown in the general formula (II): Among them, R1~R8 are the same as or different from each other, and are independently selected from hydrogen, fluorine, C1~C10 alkyl, fluorinated C1~C10 alkyl, C1~C10 ester, C1~C10 alkoxy, fluorinated C1~C10 alkoxy, C6~C30 aryl or C6~C30 aryloxy, and at least one of R1~R8 is a non-hydrogen group.
9. The method for preparing a polyimide containing a quaternary phenyl derivative structure according to claim 7, characterized in that: The inclusion The aromatic dianhydride monomer of the structure is selected from at least one of the following aromatic dianhydride monomers: 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 4,4'-oxydiphthalic anhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxylic acid)hexafluoropropane dianhydride, 4,4'-phenylenedioxydiphthalic anhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 3,3',4,4'-diphenyl sulfonetetracarboxylic dianhydride, 4,4'-(4,4'-isopropyldiphenyloxy)phthalic anhydride, and p-phenylene-diphenyltrimethylol dianhydride; Contains R B The aromatic diamine monomer of the structure is selected from at least one of the following aromatic diamine monomers: p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 4,4"-diaminoquaterphenyl, 4,4"-diaminoterphenyl, 1,3-bis(4'-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether, 2,2'-difluoro-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)diaminobiphenyl, 4,4'-diamino-2,2'-dimethyl-1,1'-biphenyl, 2 ,2'-bis[4-(4-aminophenoxyphenyl)]propane, 4,4'-diaminobenzoic acid phenyl ester, di-p-aminophenyl terephthalate, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminobiphenyl, 22'-diaminodiphenyl sulfide, 4,4-diaminodiphenyl sulfide, 4,4'-bis(3-aminophenoxy)benzophenone, 3,3',5,5'-tetramethylbenzidine, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)diphenyl sulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane.
10. A diamine monomer containing a quaternary phenyl derivative structure, having the structure shown below:
11. The method for preparing the diamine monomer containing a quaternary derivative structure according to claim 10, comprising the following steps in sequence: (1) preparing compound A2 by Miyaura borate esterification reaction of raw material A1; (2) A2 and an excess of halide A3 undergo Suzuki coupling reaction to prepare a new halide A4; (3) A4 is subjected to Suzuki reaction with phenylboronic acid or boric ester A5 having an amino group or a nitro group to prepare compound A6; (4) A6 is subjected to Suzuki reaction with phenylboronic acid or boric ester A7 having an amino group or a nitro group to prepare compound A8; (5) A8 is reduced to obtain the target product of general formula (II); The synthesis path is as follows: in, X is a halogen; Y is a borate or boric acid; Z1 and Z2 are amino or nitro groups; when compound A4 is commercially available, steps (1) and (2) are omitted; when A5 is the same as A7, steps (3) and (4) are combined into one step; when Z1 and Z2 are amino groups, step (5) is omitted, and A8 is the target product of general formula (II); When Z1 or Z2 carries a nitro group, A8 is reduced by step (5) to obtain the target product of general formula (II); wherein R1 to R8 are the same as or different from each other, and are independently selected from hydrogen, fluorine, C1 to C10 alkyl, fluorinated C1 to C10 alkyl, C1 to C10 ester, C1 to C10 alkoxy, fluorinated C1 to C10 alkoxy, C6 to C30 aryl or C6 to C30 aryloxy, and at least one of R1 to R8 is a non-hydrogen group.
12. The method for preparing a diamine monomer containing a quaternary phenyl derivative structure according to claim 11, characterized in that: In the step (1), under the protection of an inert gas, compound A1 is added to a solvent, and then pinacol diborate, a base, and a palladium catalyst are added. After the reaction, the solvent is removed, and the compound A2 is obtained by separation and purification. In the step (2), under the protection of an inert gas, compound A2 is added to a solvent, a catalytic amount of a catalyst is added, an alkali solution is added, and then compound A3 is added to react. After the reaction is completed, the liquids are separated, the solvent is removed by rotary evaporation, and the compound A4 is obtained after separation and purification. In the steps (3) and (4), under the protection of an inert gas, raw materials are added to the solvent, a catalytic amount of a catalyst is added, an alkali solution is added, and then a compound with an amino group or a nitro group is added to react. After the reaction is completed, the liquids are separated, the solvent is removed by rotary evaporation, and the corresponding product is obtained after separation and purification. In the step (5), after removing the air, the raw materials are added, and the target product of the general formula (II) is prepared by reduction reaction.
13. The method for preparing a diamine monomer containing a quaternary phenyl derivative structure according to claim 12, characterized in that: In the step (1), the solvent is one of dimethyl sulfoxide, dimethylformamide (DMF), dioxane, and toluene; the palladium catalyst is one of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride and [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride dichloromethane complex; the base is potassium carbonate, potassium phosphate or potassium acetate; and the reaction temperature is 80 to 110° C.; in the steps (2), (3) and (4), the solvent is tetrahydrofuran, dioxane, , toluene, ethanol, DMF, the catalyst is one of tetrakistriphenylphosphine palladium and triphenylphosphine / palladium acetate, the base is one of sodium carbonate, potassium carbonate, potassium phosphate, cesium fluoride, cesium carbonate, barium hydroxide and sodium hydroxide, and the reaction temperature is 65-100° C.; in step (5), the reduction reaction is a hydrogen reduction reaction catalyzed by Pd / C, a reduction reaction under Fe / dilute hydrochloric acid, a reduction reaction under stannous chloride / dilute hydrochloric acid or a hydrazine hydrate reduction reaction catalyzed by Pd / C.
Citation Information
Patent Citations
A low dielectric loss polyimide film
CN109651631B
Polyimide, polyimide precursor, and polyimide film
JP2018080315A
Thermoplastic polyimide and preparation method of two-layer process adhesive-free double-side flexible copper clad plate using thermoplastic polyimide
CN102408564A
Method for synthesizing nitrobiphenyl compound
CN103360261A
Ester group-containing tetracarboxylic dianhydride, polyimide precursor polyester, polyester imide and its manufacturing method