Liming liquid for preparing bone gelatin and preparation method of bone gelatin

By using 0.01~3mm small-particle bone particles and homogeneous ash liquor for acid-eluting calcium and homogeneous ash liquor, the problems of low freezing and low quality of traditional alkaline bone gelatin are solved, and efficient glue extraction and hydrolysis are achieved. , reduces production cycle and wastewater production, and improves product quality and utilization.

CN116478625BActive Publication Date: 2024-11-22HUARONG CHEM (CHENGDU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310386721.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-11-22
Estimated Expiration
2043-04-12

AI Technical Summary

Technical Problem

The production of traditional alkaline gelatin has problems with low freezing force and low quality gelatin, and the wastewater volume is large, the production cycle is long, and the glue extraction rate is low, resulting in high product cost and unqualified quality.

Method used

The 0.01-3mm small-particle size bone particles and homogeneous ash liquor were used for acid-eluting calcium and homogeneous ash liquor, and the ash liquor of 0.05-1.0% alkali and 0.2-3% salt were used for ash liquor, combined with 0.5 ~5% additives such as hydrogen peroxide and sodium hypochlorite achieve more complete hydrolysis and glue extraction, reduce wastewater and solid waste, and shorten production cycle.

Benefits of technology

It improves the freezing force and glue extraction rate of gelatin, shortens the production cycle, reduces the generation of wastewater and solid waste, and improves product quality and aggregate utilization.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a liming liquid for preparing bone gelatin and a preparation method of bone gelatin, and belongs to the technical field of gelatin processing. The preparation method of bone gelatin is as follows: bone particles are washed with acid and then separated into solid and liquid to obtain decalcified bone element, and then the decalcified bone element is washed with alkali solution and clean water, and then the acid-removed bone element obtained by washing is mixed with a homogeneous liming liquid for liming to obtain limed bone element, and then the limed bone element is washed with acid and clean water to obtain the delimed bone element, and then gelatin is extracted and post-processed to obtain bone gelatin. The overall freezing force and yield of the bone gelatin prepared by the method of the invention are significantly higher than those of gelatin products obtained by the existing traditional alkali method technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of gelatin processing, and particularly relates to a liming liquid for preparing bone gelatin and a preparation method of bone gelatin with high freezing strength and high yield. Background Art

[0002] Gelatin is a polymer of high molecular weight polypeptides obtained by purifying and primary hydrolyzing collagen contained in animal skin, bones, cartilage, ligaments, and fascia. In addition to a small amount of water and inorganic salts, the finished gelatin product contains more than 82% protein and is widely used in food, medicine, cosmetics, biomaterials and other fields. Bone gelatin is used for a wide range of raw materials and high product quality, and is one of the main sources of commercial high-quality gelatin.

[0003] The preparation methods of bone gelatin mainly include alkali method, acid method and enzyme method. Among them, the most traditional and widely used is alkali method. Alkaline gelatin can produce high viscosity and high freezing strength gelatin products with different requirements. The process is stable and is the mainstream process of bone gelatin. However, traditional alkali gelatin also has many problems, such as large amount of wastewater, one ton of gelatin consumes about 500~600 tons of water; long production cycle, because it uses 3~20mm bone particles for production, countercurrent extraction decalcification and 3~4% lime emulsion liming, slow reaction, long reaction time, production cycle often reaches 40~60 days; low gelatin extraction rate, compared with bone particles, the product extraction rate is generally 13~15%, and at the same time, 20~30% low freezing strength (less than 170Bloom g) gelatin or other low-quality gelatin with seriously unqualified viscosity and transparency will be produced as by-products. These low-quality gelatins can often only be sold as food grade or even industrial grade gelatin, with low prices, which compresses the profits of manufacturers.

[0004] Among the current patents for preparing bone gelatin, the patent with publication number CN103333939A discloses "a method for preparing gelatin by degrading collagen fibers with an alkali enzyme complex". The gelatin is prepared using osteoin obtained by demineralizing large bone particles (2~5cm) as a raw material. The demineralization of large bone particles is carried out using high-concentration hydrochloric acid, which severely damages the internal peptide chains of collagen fibers, making the subsequent enzymatic hydrolysis process difficult to control and the viscosity of the gelatin product too low (2-4mPa·s).

[0005] Chinese patent CN112608686A discloses a method for preparing bone gelatin by improving the traditional alkaline method, which uses saturated clear lime water instead of the traditional 3-5% lime milk to lime 5-20 mm bone particles, which can greatly reduce the waste lime milk solid waste. At the same time, it claims that the liming cycle can be shortened and the gelatin extraction rate can be increased to 13-15% (bone consumption 6.6-7 tons / ton gelatin), but it does not solve the problem of low freezing gelatin in traditional alkaline gelatin. From the examples, the gelatin freezing strength obtained in the examples and the comparative examples is 200-210 Bloomg, which should be the test value of multiple passes, and the problem of low freezing gelatin is still unsolved. In theory and actual experiments, the hydrolysis ability of saturated clear lime water on bone element is not stronger than that of traditional 3-5% lime milk, so the effect of shortening the liming cycle mentioned in the patent is also difficult to achieve. In addition, the existing alkaline gelatin technology has the problem that as the number of gelatin extraction passes increases, the quality of gelatin gradually decreases, and the final product contains 20~30% low-quality gelatin products with unqualified indicators such as freezing strength, viscosity, and transmittance. At the same time, the existing bone gelatin has a low extraction rate relative to bone particles, at 13~15%, resulting in high bone loss and high cost.

[0006] Therefore, it is urgent to develop a production process that can improve the gelatin extraction rate and freezing strength of bone gelatin. Summary of the invention

[0007] The purpose of the present invention is to provide a liming liquid for preparing bone gelatin and a preparation method of bone gelatin, so as to solve the problem that a certain proportion of low freezing strength and low quality gelatin exists in the production process of alkaline bone gelatin, while minimizing waste water, shortening the production cycle and improving the gelatin extraction rate of the overall product.

[0008] In order to solve the above technical problems, the inventors found through long-term production research that the fundamental reason for the low-quality gelatin in traditional alkaline bone gelatin is that it is difficult to fully and properly react inside the large-particle bone particles of 5-20 mm, and due to the low solubility of calcium hydroxide, it is impossible to further achieve full reaction through the concentration of ash milk, and the gelatin hydrolysis temperature is higher than 20°C, the loss is significantly increased and it is easy to breed bacteria, so it is also impossible to achieve full reaction by conventionally increasing the reaction temperature. When the particle size of the bone particles is larger, such as more than 10 mm, it is very difficult to diffuse into the bone particles for full reaction, especially when the bone particles have different soft and hard swelling differences due to different source animals and parts (such as spongy bones and heavy bones), inconsistent over-liming and under-liming will occur. Over-liming will lead to low melting and gelatin loss extraction rate, while under-liming will lead to difficulty in gelatin dissolution and extraction, and often requires increasing the temperature and extending the time. This high-temperature extraction often results in poor quality, low freezing strength, and low-quality gelatin. Similarly, it is difficult to reduce the particle size of bone particles. When the particle size is less than 5mm and the concentration of lime milk is as high as 3-5%, there is a large amount of solids as a suspension. The separation of bone particles and lime milk will face great problems. Bone particles that are too small will be discharged with each replacement of the lime liquid and cleaning. The liming process involves dozens of liming changes and cleanings. At this time, the loss of bone particles will be very large, and many bone particles cannot even complete the liming process.

[0009] To this end, the inventor proposed the following technical solution through repeated experiments and research:

[0010] In a first aspect, the present invention first provides a liming solution for preparing bone gelatin, wherein the liming solution components include 0.05-1.0% by mass of an alkali and 0.2-3% by mass of a salt; the alkali is selected from one or more of metal hydroxides, metal carbonates, and metal bicarbonates, and the salt is selected from at least one of metal chlorides and ammonium chloride.

[0011] In a specific embodiment of the present invention, the metal in the metal hydroxide, metal carbonate and metal bicarbonate is selected from one of calcium, potassium and sodium.

[0012] In a specific embodiment of the present invention, the metal in the metal chloride and metal sulfide is selected from one of calcium, sodium and potassium.

[0013] In a specific embodiment of the present invention, the mass fraction of the base is 0.2-0.4%, and the mass fraction of the salt is 0.5-1%.

[0014] In a specific embodiment of the present invention, the liming liquid component further comprises an auxiliary agent with a mass fraction of 0.5-5%, and the auxiliary agent is selected from one or more of hydrogen peroxide, hypochlorite, and tetramethyl hydroxide.

[0015] The homogeneous liming solution of the present invention is more efficient and cleaner than the traditional 3-5% lime milk liming solution. In the homogeneous liming solution, completely dissolved alkaline components such as calcium hydroxide and sodium hydroxide mainly provide the necessary alkaline conditions for hydrolyzing collagen; inorganic salts such as sodium chloride and calcium chloride that have swelling effects on collagen fibers are used as swelling components, and the swollen collagen fibers help them to be more fully and evenly hydrolyzed; the homogeneous liming solution of the present invention can also add auxiliary agents such as hydrogen peroxide, sodium hypochlorite, and tetramethylammonium hydroxide, which can play the role of oxidative decolorization and sterilization, further promote collagen hydrolysis and\or chelate heavy metal ions. The three components work synergistically, and the efficiency of lime milk liming is improved relative to that of single lime milk. Moreover, since it is a homogeneous solution, no cleaning is required when changing the ash, and no large amount of solid waste alkali is generated, wastewater and solid waste are reduced, and it is cleaner.

[0016] In a second aspect, the present invention further provides a method for preparing bone gelatin, comprising the following steps:

[0017] (1) washing the bone particles with acid and then separating the solid and liquid to obtain decalcified osteotin;

[0018] (2) washing the decalcified osteoincretin with alkali solution and clean water to obtain decalcified osteoincretin, mixing the decalcified osteoincretin with liming liquid for liming, and separating the limed osteoincretin after liming;

[0019] (3) Wash the limed bone with acid and water to obtain the delimed bone, then perform gelatin extraction and post-processing to obtain bone gelatin.

[0020] In a specific embodiment of the present invention, the particle size of the bone particles in step (1) is 0.01-3 mm.

[0021] On the basis of using a homogeneous liming solution, the present invention replaces the bone particles with a particle size of 5-20 mm in the traditional alkali method with small-particle bone particles of 0.01-3 mm, so that the bone particle liming reaction is more sufficient, and the gelatin extraction rate of 15-17% can be achieved in 1-3 passes, and the freezing strength of gelatin in all passes is higher than 180 bloomg (the freezing strength of the last pass of gelatin in the traditional alkali method is generally 120-170 bloomg). While solving the problem of low freezing strength and poor quality of the last pass of gelatin in the alkali method gelatin, the total gelatin extraction rate is also greatly improved compared with the prior art.

[0022] Furthermore, the particle size of the bone particles is preferably 0.25-1 mm.

[0023] Furthermore, the acid in step (1) is selected from one or more of hydrochloric acid, phosphoric acid, and organic acid;

[0024] Furthermore, the mass fraction of the acid is 1-5 wt %;

[0025] Furthermore, the pickling time is 2 to 5 hours.

[0026] In a specific embodiment of the present invention, the alkali in the alkali solution in step (2) is selected from one or more of calcium hydroxide, sodium hydroxide and potassium hydroxide;

[0027] Furthermore, the mass fraction of the alkali is 0.1-10%;

[0028] Further, the decalcified osteoin is washed with alkali solution and clean water until the pH value is 5-8 to obtain deacidified osteoin;

[0029] Furthermore, the mass ratio of the liming liquid to the osteoblastic acid is 4-8:1.

[0030] In a specific embodiment of the present invention, the liming conditions are: liming at 8-27°C for 15-45 days; further, liming at 10-20°C for 20-40 days;

[0031] Further, the liming system is circulated with liming liquid and / or stirred at a speed not higher than 80 r / min for 5 to 10 min every 4 to 8 hours;

[0032] Furthermore, the liming solution is replaced every 2 to 7 days and / or when the COD of the liming solution is greater than 3000 mg / L.

[0033] Furthermore, when the liming liquid is replaced, a centrifugal or filtering device is used to separate the liming liquid and the osteoin, and the separated osteoin is returned to the liming device, and new homogeneous liming liquid is added; the centrifugal or filtering device is selected from at least one of a sedimentation centrifuge, a bag centrifuge, a plate and frame filter press, and a vacuum filter.

[0034] In a specific embodiment of the present invention, the acid in step (3) is selected from one or more of hydrochloric acid, phosphoric acid, and organic acid; further, the organic acid is selected from one or more of formic acid, acetic acid, propionic acid, and oxalic acid;

[0035] Further, the limed bone is washed with acid and water until the pH value is 4-6 to obtain the delimed bone.

[0036] In a specific embodiment of the present invention, the steps of extracting the glue are: extracting the glue for 1 to 3 times at 55 to 90° C., each time for 2 to 3 hours, adding clean water after each time of extracting the glue to enter the next time of extracting the glue;

[0037] Furthermore, the mass ratio of clean water to osteocalcin is 1-10:1; furthermore, it is 1-5:1.

[0038] Furthermore, the temperature of each glue extraction step is gradually increased.

[0039] In a specific embodiment of the present invention, the post-treatment steps in step (3) include but are not limited to filtration, ion exchange, sterilization, concentration, molding, drying, etc.

[0040] The invention has the following beneficial effects: the invention uses the technology of acid washing and decalcification of small-size bone particles of 0.01-3 mm + homogeneous liming + 1-3 times of glue extraction to greatly shorten the production cycle of alkaline gelatin; the traditional alkaline gelatin uses bone particles of 5-20 mm, and acid washing and decalcification adopts countercurrent extraction with a cycle of about 7-15 days, while the invention uses small-size bone particles for acid washing, and decalcification only takes 2-5 hours; the traditional alkaline liming cycle is 40-60 days, while the small-size homogeneous liming cycle of the invention is about 20-40 days, and the liming cycle is greatly shortened; the traditional alkaline gelatin needs to be subjected to multiple glue extractions of 4-6 times, while the glue extraction of the invention does not exceed 3 times, and while the operation time is shortened, the glue extraction rate and the freezing force are improved as a whole. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0043] It should be understood that the experimental methods used in the following examples are conventional methods unless otherwise specified, and the materials, reagents, etc. used in the following examples are all commercially available unless otherwise specified.

[0044] As used herein, the terms "comprises," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, or article that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, or article.

[0045] In the embodiments of the present invention, the implementation conditions not mentioned maintain the same operating conditions, methods or requirements as the existing traditional alkaline industrial production, such as the bone particles used are defatted bone particles with residual fat less than 2% after defatting, the water used for gelatin extraction is industrial pure water, and the analysis methods of indicators such as gelatin freezing force, viscosity, and transmittance are methods well known to those skilled in the art.

[0046] The detection data in the embodiments of the present invention are all average values.

[0047] Example 1

[0048] S1: acid washing and decalcification: 10 kg of bone particles with a particle size of 0.01-0.25 mm were stirred and acid washed and decalcified in 3w% dilute hydrochloric acid for 2 hours, and decalcified bone was separated using a sedimentation centrifuge;

[0049] S2: washing and deacidification: washing the decalcified osteotin obtained in S1 with 0.1% calcium hydroxide solution and clean water until the pH is 5, to obtain deacidified osteotin;

[0050] S3: Homogeneous liming: Mix the deacidified bone essence obtained in S2 with homogeneous liming solution (alkali: 10℃ saturated calcium hydroxide solution + 0.2% NaOH; salt: 0.5% CaCl2, auxiliary agent: 5% hydrogen peroxide) for liming, the mass ratio of liming solution to deacidified bone essence is 4:1, liming at 10-12℃ for 20 days, circulate the liming solution for 5 minutes every 4 hours, replace the homogeneous liming solution every 2 days and when the COD of the homogeneous liming solution is >3000mg / L, and separate and obtain the limed bone essence after liming;

[0051] S4: washing and deliming: washing the limed bone element obtained in S3 with 5% dilute hydrochloric acid and clean water until the pH value is 4, and obtaining delimed bone element;

[0052] S5: gelatin extraction and post-treatment: add the bone extract obtained in S4 to clean water (water: bone extract mass ratio = 5:1), extract gelatin once at 70℃, release gelatin after 3h, filter the gelatin solution through cotton cake to remove large particle suspension to obtain dilute gelatin solution. The dilute gelatin solution is further filtered through diatomaceous earth, cardboard filter and ultrafiltration to remove fine impurities to obtain fine filtered gelatin solution, and the fine filtered gelatin solution is exchanged and removed through ion exchange resin to obtain purified gelatin solution, and the purified gelatin solution is sterilized at 138~146℃ for 5S. After sterilization, the gelatin solution is concentrated to 25~35%, and sent to the gelatin extruder for molding and extrusion. The extruded gelatin strip is dried and crushed in a long-net dryer to obtain 1531.66g of gelatin, with a relative bone particle extraction rate of 15.32%. The sample test shows that the freezing strength is 229Blommg and the viscosity is 4.83mPa·s.

[0053] Example 2

[0054] S1: acid washing and decalcification: 78.6 kg of bone particles with a particle size of 0.25-1 mm were stirred and acid washed and decalcified in 4w% dilute hydrochloric acid for 3 hours, and centrifuged to obtain decalcified bone minerals;

[0055] S2: washing and deacidification: washing the decalcified osteotin obtained in S1 with 1% sodium hydroxide solution and clean water to a pH of 6 to obtain deacidified osteotin;

[0056] S3: Homogeneous liming: Mix the deacidified bone essence obtained in S2 with homogeneous liming liquid (alkali: 0.3% NaOH + 0.05% calcium hydroxide solution; salt: 0.9% NaCl) for liming, the mass ratio of liming liquid to deacidified bone essence is 4:1, liming at 10-12°C for 30 days, the homogeneous liming liquid is at least 20cm higher than the bone essence during the liming process, the liming system is stirred at no more than 60r / min for 5min every 5h, and the homogeneous liming liquid is replaced every 2d or when the COD of the homogeneous liming liquid is >3000mg / L, and the limed bone essence is separated after liming;

[0057] S4: washing and deliming: washing the limed bone element obtained in S3 with 10% dilute phosphoric acid and clean water until the pH value is 5, and obtaining delimed bone element;

[0058] S5: gelatin extraction and post-processing: add the bone extract obtained in S4 into clean water (mass ratio of clean water: bone extract = 2:1), extract at 65℃ and 75℃ respectively, for 2 times in total, each time for 3h, filter the large suspended particles of the gelatin solution through cotton cake to obtain a dilute gelatin solution in each time, further filter the fine impurities through diatomaceous earth, cardboard filter and ultrafiltration to obtain a fine filtered gelatin solution, and remove the inorganic salts through ion exchange resin to obtain a purified gelatin solution, and keep the purified gelatin solution at 138-146℃ for 5S for sterilization. After sterilization, the gelatin solution is concentrated to 25-35% and sent to a gelatin extruder for extrusion. The extruded gelatin strips are dried and crushed in a long mesh dryer to obtain the first and second gelatin products respectively.

[0059] Among them, 8.60kg of gelatin was obtained in the first coat, and the tested freezing strength was 242Bloomg; 4.63kg of gelatin was obtained in the second coat, and the tested freezing strength was 219Bloomg; the total gelatin extraction rate relative to bone particles was 16.84%, and the viscosity, transmittance and other indicators of the last coat of gelatin (the second coat of gelatin) were tested: the viscosity was 3.75mPa·s, the transmittance at 450nm: 75%; the transmittance at 620nm: 85%, which met the relevant indicator requirements of the medicinal gelatin standard QB2354-2005.

[0060] Example 3

[0061] S1: acid washing and decalcification: 78.6 kg of bone particles with a particle size of 0.25-1 mm were stirred and acid washed and decalcified in 4w% dilute hydrochloric acid for 3 hours, and decalcified bone was obtained by centrifugation;

[0062] S2: washing and deacidification: washing the decalcified osteotin obtained in S1 with 1% sodium hydroxide solution and clean water until the pH is 7 to obtain deacidified osteotin;

[0063] S3: Homogeneous liming: Mix the deacidified bone essence obtained in S2 with homogeneous liming solution (alkali: 0.3% NaOH; salt: 0.9% NaCl, additive: 2% hydrogen peroxide + 0.5% calcium hypochlorite) for liming, the mass ratio of liming solution to deacidified bone essence is 4:1, liming at 15-18°C for 30 days, the homogeneous liming solution is at least 20cm higher than the bone essence during the liming process, the liming system is stirred at no more than 60r / min for 5min every 4h, and the homogeneous liming solution is replaced every 2d or when the COD of the homogeneous liming solution is>3000mg / L, and the limed bone essence is separated after liming;

[0064] S4: washing and deliming: washing the limed bone element obtained in S3 with 10% dilute phosphoric acid and clean water until the pH value is 6, and obtaining delimed bone element;

[0065] S5: gelatin extraction and post-processing: add the bone extract obtained in S4 into clean water (mass ratio of clean water: bone extract = 2:1), extract at 65℃ and 75℃ respectively, for 2 times in total, each time for 3h, filter the large suspended particles of the gelatin solution through cotton cake to obtain a dilute gelatin solution in each time, further filter the fine impurities through diatomaceous earth, cardboard filter and ultrafiltration to obtain a fine filtered gelatin solution, and remove the inorganic salts through ion exchange resin to obtain a purified gelatin solution, and keep the purified gelatin solution at 138-146℃ for 5S for sterilization. After sterilization, the gelatin solution is concentrated to 25-35% and sent to a gelatin extruder for extrusion. The extruded gelatin strips are dried and crushed in a long-net dryer to obtain the first and second gelatin products respectively.

[0066] Among them, 6.80kg of gelatin was obtained in the first pass, and the tested freezing strength was 312Bloomg; 5.86kg of gelatin was obtained in the second pass, and the tested freezing strength was 202Bloomg; the total gelatin extraction rate relative to bone particles was 16.11%.

[0067] The viscosity, transmittance and other indicators of the last coat of glue (the second coat of glue) were tested: the viscosity was 4.20mPa·s, the transmittance at 450nm: 85%; the transmittance at 620nm: 95%, which met the relevant indicator requirements of the pharmaceutical gelatin standard QB2354-2005.

[0068] From the product analysis of Example 2 and Example 3, it can be seen that a higher yield of bone gelatin can be obtained by using the homogeneous liming solution containing components A and B, but the product obtained in the presence of additive C (such as 2% hydrogen peroxide + 0.5% calcium hypochlorite) has better indicators such as viscosity and transmittance, and the product quality is higher.

[0069] Example 4

[0070] S1: acid washing and decalcification: 58.7 kg of bone particles with a particle size of 0.5-1 mm were stirred and acid washed and decalcified in 4% dilute hydrochloric acid for 3 hours, and centrifuged to obtain decalcified bone minerals;

[0071] S2: washing and deacidification: washing the decalcified osteotin obtained in S1 with 1% sodium hydroxide solution and clean water to pH=8 to obtain deacidified osteotin;

[0072] S3: Homogeneous liming: Mix the deacidified bone essence obtained in S2 with homogeneous liming solution (alkali: 0.3% NaOH+0.1NaHCO3; salt: 0.5% CaCl2, auxiliary agent: 1% sodium hypochlorite+0.5% tetramethylammonium hydroxide) for liming, the mass ratio of liming solution to deacidified bone essence is 4:1, liming at 18-20℃ for 40 days, the homogeneous liming solution is at least 20cm higher than the bone essence during the liming process, the liming system is stirred at no more than 60r / min for 5min every 4h, and the homogeneous liming solution is replaced every 2d or when the COD of the homogeneous liming solution is>3000mg / L, and the limed bone essence is separated after liming;

[0073] S4: washing and deliming: washing the limed bone element obtained in S3 with 10% dilute phosphoric acid and clean water until the pH value is 5, and obtaining delimed bone element;

[0074] S5: gelatin extraction and post-processing: add the bone extract obtained in S4 into clean water (mass ratio of clean water: bone extract = 2:1), extract at 60℃, 70℃ and 80℃ respectively, for a total of 3 times, each time for 2h, filter the large suspended particles of the gelatin solution through cotton cake to obtain a dilute gelatin solution in each time, further filter the fine impurities through diatomaceous earth, cardboard filter and ultrafiltration to obtain a fine filtered gelatin solution, and remove the inorganic salts from the fine filtered gelatin solution through ion exchange resin to obtain a purified gelatin solution, and keep the purified gelatin solution at 138-146℃ for 5S for sterilization. After sterilization, the gelatin solution is concentrated to 25-35% and sent to a gelatin extruder for molding and extrusion. The extruded gelatin strips are dried and crushed in a long-net dryer to obtain 1-3 gelatin products respectively.

[0075] Among them, 4.17 kg of gelatin was obtained in the first pass, and the tested freezing force was 252 Bloomg; 2.70 kg of gelatin was obtained in the second pass, and the tested freezing force was 211 Bloomg; 1.95 kg of gelatin was obtained in the third pass, and the tested freezing force was 198 Bloomg, and the total gelatin extraction rate relative to the bone particles was 15.07%; and the viscosity, transmittance and other indicators of the last pass of gelatin (the third pass of gelatin in this embodiment) were tested: the viscosity was 4.25 mPa·s, the transmittance at 450nm: 80%; the transmittance at 620nm: 90%, which met the relevant indicator requirements of the pharmaceutical gelatin standard QB2354-2005.

[0076] Example 5

[0077] S1: acid washing and decalcification: 66.56 kg of bone particles with a particle size of 1-3 mm were stirred and acid washed and decalcified in 3.5w% dilute hydrochloric acid for 5 hours, and centrifuged to obtain decalcified bone minerals;

[0078] S2: washing and deacidification: washing the decalcified osteotin obtained in S1 with 10% sodium hydroxide solution and clean water to a pH of 6 to obtain deacidified osteotin;

[0079] S3: Homogeneous liming: Mix the deacidified bone essence obtained in S2 with homogeneous liming solution (alkali: 0.4% KOH+1% K2CO3; salt: 1% CaCl2, additive: 4% hydrogen peroxide + 0.5% tetramethylammonium hydroxide) for liming, the mass ratio of liming solution to deacidified bone essence is 4:1, liming is carried out at 25-27℃ for 40 days, the homogeneous liming solution is higher than the bone essence by more than 20cm during the liming process, the liming system is stirred at no more than 80r / min for 5min every 8h, and the homogeneous liming solution is replaced every 2d or when the COD of the homogeneous liming solution is>3000mg / L, and the limed bone essence is separated after liming is completed;

[0080] S4: washing and deliming: washing the limed bone element obtained in S3 with 10% dilute phosphoric acid and clean water until the pH value is 6, and obtaining delimed bone element;

[0081] S5: gelatin extraction and post-processing: add the bone extract obtained in S4 into clean water (mass ratio of clean water: bone extract = 3:1), extract at 65℃, 75℃ and 85℃ respectively, for 3 times in total, each time for 2h, filter the large suspended particles of the gelatin solution through cotton cake to obtain a dilute gelatin solution in each time, further filter the fine impurities through diatomaceous earth, cardboard filter and ultrafiltration to obtain a fine filtered gelatin solution, and remove the inorganic salts from the fine filtered gelatin solution through ion exchange resin to obtain a purified gelatin solution, and keep the purified gelatin solution at 138-146℃ for 5S for sterilization. After sterilization, the gelatin solution is concentrated to 25-35% and sent to a gelatin extruder for molding and extrusion. The extruded gelatin strips are dried and crushed in a long-net dryer to obtain 1-3 gelatin products respectively.

[0082] Among them, 5.28kg of gelatin was obtained in the first pass, and the tested freezing strength was 246Bloomg; 3.08kg of gelatin was obtained in the second pass, and the tested freezing strength was 211Blommg; 2.64kg of gelatin was obtained in the third pass, and the tested freezing strength was 185Bloomg; the total gelatin extraction rate relative to bone particles was 16.53%.

[0083] Example 6

[0084] S1: acid washing and decalcification: 5.22 kg of bone particles with a particle size of 0.25-1 mm were stirred and acid washed and decalcified in 4w% dilute hydrochloric acid for 3 hours, and centrifuged to obtain decalcified bone minerals;

[0085] S2: washing and deacidification: washing the decalcified osteotin obtained in S1 with 1% sodium hydroxide solution and clean water until the pH is 7 to obtain deacidified osteotin;

[0086] S3: Homogeneous liming: Mix the deacidified bone essence obtained in S2 with a homogeneous liming solution (alkali: 0.5% sodium carbonate + 0.2% NaOH; salt: 0.9% NaCl, additive: 2% hydrogen peroxide + 1% calcium hypochlorite) for liming, the mass ratio of liming solution to deacidified bone essence is 4:1, liming at 10-15°C for 30 days, the homogeneous liming solution is at least 20cm higher than the bone essence during the liming process, the liming system is stirred at no more than 60r / min for 5min every 4h, and the homogeneous liming solution is replaced every 2d or when the COD of the homogeneous liming solution is >3000mg / L, and the limed bone essence is separated after liming;

[0087] S4: washing and deliming: washing the limed bone element obtained in S3 with 10% dilute phosphoric acid and clean water until the pH value is 5, and obtaining delimed bone element;

[0088] S5: gelatin extraction and post-processing: add the bone extract obtained in S4 into clean water (mass ratio of clean water: bone extract = 2:1), extract at 65℃ and 75℃ respectively, for 2 times in total, each time for 3h, filter the large suspended particles of the gelatin solution through cotton cake to obtain a dilute gelatin solution in each time, further filter the fine impurities through diatomaceous earth, cardboard filter and ultrafiltration to obtain a fine filtered gelatin solution, and remove the inorganic salts through ion exchange resin to obtain a purified gelatin solution, and keep the purified gelatin solution at 138-146℃ for 5S for sterilization. After sterilization, the gelatin solution is concentrated to 25-35% and sent to a gelatin extruder for extrusion. The extruded gelatin strips are dried and crushed in a long-net dryer to obtain the first and second gelatin products respectively.

[0089] Among them, 550.23g of gelatin was obtained in the first pass, and the tested freezing strength was 234Bloomg; 395.48g of gelatin was obtained in the second pass, and the tested freezing strength was 222Blommg; the total gelatin extraction rate relative to bone particles was 16.47%.

[0090] Example 7

[0091] S1: acid washing and decalcification: 10 kg of bone particles with a particle size of 0.01-0.25 mm were stirred and acid washed and decalcified in 1w% dilute hydrochloric acid for 2 hours, and decalcified bone was separated using a sedimentation centrifuge;

[0092] S2: washing and deacidification: washing the decalcified osteotin obtained in S1 with 10% potassium hydroxide solution and clean water to pH = 8 to obtain deacidified osteotin;

[0093] S3: Homogeneous liming: Mix the deoxidized bone essence obtained in S2 with homogeneous liming solution (alkali: 1% potassium hydroxide + 0.05% NaOH; salt: 3% CaCl2, auxiliary agent: 5% sodium hypochlorite) for liming, the mass ratio of liming solution to deoxidized bone essence is 8:1, liming at 8-12℃ for 45 days, stirring the liming system at no more than 80r / min for 10 minutes every 4-8 hours, replacing the homogeneous liming solution every 7 days and when the COD of the homogeneous liming solution is>3000mg / L, and separating and obtaining the limed bone essence after liming;

[0094] S4: washing and deliming: washing the limed bone essence obtained in S3 with 5% dilute hydrochloric acid and clean water until the pH value is 5, and obtaining delimed bone essence.

[0095] S5: gelatin extraction and post-treatment: add the bone extract obtained in S4 to clean water (water: bone extract mass ratio = 10:1), extract gelatin once at 90℃, release gelatin after 3h, filter the gelatin solution through cotton cake to remove large particle suspension to obtain dilute gelatin solution. The dilute gelatin solution is further filtered through diatomaceous earth, cardboard filter and ultrafiltration to remove fine impurities to obtain fine filtered gelatin solution, and the fine filtered gelatin solution is exchanged and removed through ion exchange resin to obtain purified gelatin solution, and the purified gelatin solution is sterilized at 138-146℃ for 5S. After sterilization, the gelatin solution is concentrated to 25-35%, and sent to the gelatin extruder for extrusion. The extruded gelatin strip is dried and crushed in a long net dryer to obtain 1505.35g of gelatin, with a relative bone particle extraction rate of 15.05%. The freezing strength of the sample test is 199Blommg and the viscosity is 4.31mPa·s.

[0096] Example 8

[0097] S1: acid washing and decalcification: 78.6 kg of bone particles with a particle size of 0.25-1 mm were stirred and acid washed and decalcified in 5w% dilute hydrochloric acid for 3 hours, and centrifuged to obtain decalcified bone minerals;

[0098] S2: washing and deacidification: washing the decalcified osteotin obtained in S1 with 5% sodium hydroxide solution and clean water to a pH of 6 to obtain deacidified osteotin;

[0099] S3: Homogeneous liming: Mix the deacidified bone essence obtained in S2 with homogeneous liming liquid (alkali: 1.0% NaOH; salt: 0.2% NaCl) for liming, the mass ratio of liming liquid to deacidified bone essence is 4:1, liming at 20-27°C for 15 days, the homogeneous liming liquid is at least 20 cm higher than the bone essence during the liming process, the liming system is stirred at no more than 60 r / min for 5 minutes every 4 hours, and the homogeneous liming liquid is replaced every 2 days or when the COD of the homogeneous liming liquid is >3000 mg / L, and the limed bone essence is separated after liming is completed;

[0100] S4: washing and deliming: washing the limed bone element obtained in S3 with 10% dilute phosphoric acid and clean water until the pH value is 4, and obtaining delimed bone element;

[0101] S5: gelatin extraction and post-processing: add the bone extract obtained in S4 into clean water (mass ratio of clean water: bone extract = 1:1), extract at 60℃ and 80℃ respectively, for 2 times in total, each time for 3h, filter the large suspended particles of the gelatin solution through cotton cake to obtain a dilute gelatin solution in each time, further filter the fine impurities through diatomaceous earth, cardboard filter and ultrafiltration to obtain a fine filtered gelatin solution, and remove the inorganic salt from the fine filtered gelatin solution through ion exchange resin to obtain a purified gelatin solution, and keep the purified gelatin solution at 138-146℃ for 5S for sterilization. After sterilization, the gelatin solution is concentrated to 25-35% and sent to a gelatin extruder for forming and extrusion. The extruded gelatin strips are dried and crushed in a long-net dryer to obtain the first and second gelatin products respectively.

[0102] Among them, 8.10kg of gelatin was obtained in the first coat, and the tested freezing strength was 212Bloomg; 4.15kg of gelatin was obtained in the second coat, and the tested freezing strength was 199Bloomg; the total gelatin extraction rate relative to bone particles was 15.58%, and the viscosity, transmittance and other indicators of the last coat of gelatin (the second coat of gelatin) were tested: the viscosity was 3.34mPa·s, the transmittance at 450nm: 74%; the transmittance at 620nm: 83%, which met the relevant indicator requirements of the medicinal gelatin standard QB2354-2005.

[0103] Comparative Example 1

[0104] The same implementation conditions as in Example 5 were used, except that the homogeneous liming solution in step S3 (alkali: 0.4% KOH+1% K2CO3; salt: 1% CaCl2, additive: 4% hydrogen peroxide + 0.5% tetramethylammonium hydroxide) was replaced with saturated clear lime water at 10°C, and the feed amount was changed to 5 kg.

[0105] Finally, 177.41g of gelatin was obtained in the first pass, and the tested freezing strength was 248Bloomg; 110.86g of gelatin was obtained in the second pass, and the tested freezing strength was 205Blommg; 155.23g of gelatin was obtained in the third pass, and the tested freezing strength was 185Bloomg; the total gelatin extraction rate relative to bone particles was 8.87%.

[0106] From the experimental results of Example 5 and Comparative Example 1, it can be seen that compared with liming with the homogeneous liming liquid of the present invention, although the freezing force of gelatin after three passes does not change much, the gelatin extraction rate of Example 5 is 16.53%, while the gelatin extraction rate of Comparative Example 1 is 8.87%. Obviously, the homogeneous liming liquid of Example 5 hydrolyzes bone granules more fully than the single clear lime water.

[0107] Comparative Example 2 Bone particles with a particle size of 10 mm were prepared using the traditional alkali method.

[0108] Gelatin was prepared using 10 mm defatted bone particles and 3% lime milk according to the traditional alkali method. The specific steps are as follows:

[0109] 5 kg of 10 mm defatted bone particles were subjected to countercurrent extraction and acid decalcification at 10-20°C for 72 h to obtain decalcified bone minerals.

[0110] Neutralize decalcified osteoin with dilute alkali and wash with clean water until the pH of osteoin is 5-8;

[0111] Step (2) bone essence is mixed with 3% lime milk, and limed at 10-20°C. Compressed air is blown in every 8 hours to fully stir the mixture. The lime milk is replaced every 1, 3, 5, 7, 9, ... days (every two days) or when the liming liquid turns yellow. During the liming replacement process, the mixture is washed with clean water for 1 to 3 times. The liming is carried out until the bone essence turns white, soft, tough and has a slight ammonia smell.

[0112] Use dilute hydrochloric acid and clean water to neutralize and wash osteoin to pH = 5~8. Since osteoin is relatively large, acid-washing osteoin needs to be maintained for 8~24 hours until the pH of the system stabilizes.

[0113] Use dilute phosphoric acid to adjust the pH value of osteoin to 4-5, add clean water (for the control, add 2 times the volume of osteoin), and perform 1-4 times of gelatin extraction at 60, 70, 80, and 90° C. for 3 hours respectively. The extracted gelatin solution is treated in the same way as the post-treatment method in the above embodiment to obtain 1-4 times of gelatin.

[0114] Finally, 222.01g of gelatin was obtained in the first pass, and the tested freezing strength was 246 Bloomg; 134.26g of gelatin was obtained in the second pass, and the tested freezing strength was 210 Bloomg; 143.21g of gelatin was obtained in the third pass, and the tested freezing strength was 185 Bloomg; 187.65g of gelatin was obtained in the fourth pass, and the tested freezing strength was 165 Bloomg. The total gelatin extraction rate of gelatin in passes 1 to 4 relative to bone particles was 13.74%.

[0115] Similarly, other key indicators of the final gelatin (the fourth gel) were also tested: viscosity 3.2 mPa·s, 450nm transmittance: 65%, 620nm transmittance: 80%.

[0116] Comparison of the results of Example 4 with those of Comparative Example 2 shows that Example 4 uses bone particles with a particle size of 0.5-1 mm as raw materials, and in the presence of a homogeneous liming solution (alkali: 0.3% NaOH+0.1NaHCO3; salt: 0.5% CaCl2, additive: 1% sodium hypochlorite+0.5% tetramethylammonium hydroxide), the gelatins obtained in the first to third passes are:

[0117] The first pass of gelatin was 5.17kg, and the test freezing force was 252Bloomg; the second pass of gelatin was 3.10kg, and the test freezing force was 211Blommg; the third pass of gelatin was 2.07kg, and the test freezing force was 198Bloomg. The viscosity and transmittance of the last pass of gelatin were tested: the viscosity was 4.25mPa·s, the transmittance at 450nm: 80%; the transmittance at 620nm: 90%; the total gelatin extraction rate relative to bone particles was 17.61%.

[0118] Obviously, the total gelatin extraction rate of Example 4 is 17.61%, which is higher than the total gelatin extraction rate of the comparative example 13.74%; at the same time, the freezing force of the third gelatin layer (the last gelatin layer) of Example 3 is significantly higher than the freezing force of the third and fourth gelatin layers obtained in the comparative example 2, and is higher than 180 Bloomg, and the viscosity and transmittance indexes are also higher than those of the last gelatin layer obtained in the comparative example 2.

[0119] In summary, using the method of the embodiment of the present invention, the freezing force and yield of the bone gelatin obtained are significantly higher than the gelatin product obtained by the existing traditional alkaline method, which is beneficial to improving product quality and aggregate utilization. At the same time, the preparation process cycle of the present invention is shorter, decalcification only takes 2 to 5 hours, and the liming cycle is about 20 to 40 days.

[0120] The foregoing examples are merely illustrative and are used to explain some features of the method of the present invention. The appended claims are intended to claim the widest possible range that can be conceived, and the embodiments presented herein are only illustrations of selected implementations according to the combination of all possible embodiments. Therefore, it is the applicant's intention that the appended claims are not limited by the selection of examples that illustrate the features of the present invention. Some numerical ranges used in the claims also include sub-ranges within them, and changes in these ranges should also be interpreted as being covered by the appended claims where possible.

Claims

1. A method for preparing bone gelatin, characterized in that: The steps include: (1) washing the bone particles with acid and then separating the solid and liquid to obtain decalcified osteotin; The particle size of the bone particles is 0.01 to 3 mm; The acid in step (1) is selected from one or more of hydrochloric acid, phosphoric acid, and organic acid; The mass fraction of the acid in step (1) is 1 to 5 wt%; The pickling time is 2 to 5 hours; (2) washing the decalcified osteoin with alkali solution and clean water until the pH value is 5-8 to obtain decalcified osteoin, mixing the decalcified osteoin with liming liquid for liming, and separating the limed osteoin after liming; The liming solution comprises 0.05-1.0% by mass of alkali and 0.2-3% by mass of salt; the alkali is selected from one or more of metal hydroxides, metal carbonates, and metal bicarbonates, and the salt is selected from at least one of metal chlorides and ammonium chloride; the liming solution also comprises 0.5-5% by mass of an auxiliary agent, and the auxiliary agent is selected from one or more of hydrogen peroxide, hypochlorite, and tetramethyl hydroxide; The metal in the metal hydroxide, metal carbonate, or metal bicarbonate is selected from one or more of calcium, potassium, and sodium; the metal in the metal chloride is selected from one or more of calcium, sodium, and potassium; The alkali in the alkali solution in step (2) is selected from one or more of calcium hydroxide, sodium hydroxide and potassium hydroxide; The mass fraction of the alkali in step (2) is 0.1 to 10%; The mass ratio of the liming liquid to the osteoblastic acid is 4 to 8:1; The liming conditions are: liming at 8-27°C for 15-45 days; circulating the liming liquid and / or stirring the liming system at a speed not higher than 80r / min for 5-10min every 4-8h; Replace the liming liquid every 2-7 days and / or when the COD of the liming liquid is >3000mg / L; (3) washing the limed bone with acid and water until the pH is 4-6 to obtain limed bone, and then extracting and post-processing the limed bone to obtain bone gelatin; The steps of glue extraction are: glue extraction 1 to 3 times at 60 to 90°C, each time for 2 to 3 hours, adding clean water after each glue extraction to enter the next glue extraction; The acid in step (3) is selected from one or more of hydrochloric acid, phosphoric acid, and organic acid; The organic acid is selected from one or more of formic acid, acetic acid, propionic acid and oxalic acid.

2. The method for preparing bone gelatin according to claim 1, characterized in that: The mass fraction of the alkali is 0.2-0.4%, and the mass fraction of the salt is 0.5-1%.

3. The method for preparing bone gelatin according to claim 1, characterized in that: The liming conditions are: liming at 10-20° C. for 20-40 days.

4. The preparation method according to claim 1, characterized in that: The mass ratio of clean water to decalcified bone is 1-10:

1.

5. The preparation method according to claim 4, characterized in that: The mass ratio of clean water to decalcified bone is 1 to 5:1.