A kind of steel for high-speed motor vehicle gearbox bearing and its manufacturing method

Through the new component design and optimization of vacuum degassing continuous casting process, the purity and mechanical properties of high-speed EMU gearbox bearing steel have been improved, the problem of limited pace of domestic production has been solved, and the efficient production and quality improvement of domestic bearing steel has been achieved. The goal of replacing imported materials.

CN116479322BActive Publication Date: 2024-11-15JIANGYIN XINGCHENG SPECIAL STEEL WORKS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310222340.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-09
Publication Date
2024-11-15
Estimated Expiration
2043-03-09

AI Technical Summary

Technical Problem

The purity, mechanical properties and hardenability of my country's high-speed EMU gearbox bearing steel has not yet reached the advanced level abroad, resulting in limited pace of domestic production. It is necessary to improve the process control level of vacuum degassing continuous casting process to replace imported materials.

Method used

Carburized bearing steel material designed with new components can improve the purity and structural uniformity of the steel through innovative optimization of vacuum degassing, continuous casting and rolling processes, thereby improving mechanical properties and hardenability, and meeting the high-speed EMU gearbox Quality requirements for bearings. Specific processes include KR molten pretreatment, converter or electric furnace initial refining, refining furnace refining, vacuum degassing, continuous casting, slow cooling and heating rolling, etc., combined with special smelting processes such as nitrogen and oxygen composite gas dephosphorization, active slag-forming agent Removal of harmful elements, full-process argon gas protective casting and large-pressure rolling technology.

Benefits of technology

It has achieved high purity, uniformity and mechanical properties of steel, extended fatigue life, reached advanced foreign level, shortened production cycle, improved production efficiency and cost competitiveness, and realized the domestic production of high-speed EMU gearbox bearing materials. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to a steel for a high-speed motor vehicle gearbox bearing and a manufacturing method thereof. The chemical composition is as follows: C: 0.20-0.25, Si: 0.35-0.45, Mn: 0.75-0.95, Cr: 0.80-0.90, Mo: 0.25-0.35, Ni: 1.75-2.05, Cu: 0.10-0.15, Nb: 0.06-0.10, V: 0.08-0.12, Al≤0.05, P≤0.015, S≤0.005, Ca≤0.0005, Ti≤0.0015, O≤0.0008, H≤0.0002, As≤0.010, Sn≤0.010, Sb≤0.005, Pb≤0.0015, and the remainder is Fe. The process flow is hot metal pretreatment → primary refining → refining → vacuum degassing → continuous casting → slow cooling → hot rolling → finishing. The bearing steel of this application is different from the new carburized bearing steel material listed in the current national standard GB / T 3203. Through innovative optimization in vacuum degassing, continuous casting and rolling processes, the purity and uniformity of the steel are improved, thereby improving the mechanical properties and hardenability of the steel, making the steel more impact-resistant, so that it meets the quality requirements of high-speed train gearbox bearing steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and more specifically relates to bearing steel and a production method thereof. Background Art

[0002] With the development of high-speed trains in my country, China's high-speed trains are at the forefront of the world in terms of operating mileage and speed. At present, there are still many large and medium-sized cities without high-speed rail. Compared with the huge demand for passenger transport, the gap is large. Therefore, from the perspective of passenger transport, my country's railway transportation capacity is far from enough, and it is still necessary to vigorously develop high-speed rail passenger transport.

[0003] The running gear of a high-speed EMU, i.e. the bogie, is the core component to ensure the high-speed, safe and smooth operation of the train, and bearings are one of the key parts. High-speed EMU bearings are mainly composed of axle box bearings, gear box bearings and traction motor bearings. High-speed EMU gearbox bearings are important transmission components of high-speed EMUs. Since they bear the gear meshing force and multi-directional vibration and impact of the track, the force is complex. If the high-speed EMU is to be ensured to run at high speed, safely and smoothly, the gearbox bearings are required to have high fatigue life and high impact resistance. Therefore, strict requirements are also put forward for the raw material bearing steel for manufacturing gearbox bearings. The high-speed EMU gearbox bearing material is required to have higher properties such as purity, mechanical properties, and hardenability than ordinary freight passenger car bearing materials. At present, well-known bearing steel manufacturers such as Sweden's OVAKO and Japan's Sanyo have been using high-cleanliness and high-mechanical properties vacuum degassing continuous casting process routes to produce steel that meets the requirements of high-speed train gear bearings. However, it has been difficult to produce steel with vacuum degassing continuous casting process in China, but electroslag remelting or vacuum degassing + vacuum consumable process is used to improve the quality of steel. However, the process is complicated, the production efficiency is low, and the cost is much higher than the market, making it difficult to form competitiveness. As a result, my country's high-speed train gearbox bearing steel basically needs to be imported from abroad, which greatly restricts the pace of localization of my country's high-speed train bearings.

[0004] Although my country has made great progress in the production of bearing steel using the vacuum degassing continuous casting process in recent years, there is still a certain gap with advanced foreign bearing steel manufacturers, especially in terms of control technology in terms of purity, mechanical properties and hardenability. Application No. 201710982084.7 discloses a carburized bearing steel for railway freight cars and a preparation method thereof. The steel used in freight cars is produced using the vacuum degassing continuous casting process, but its product purity, mechanical properties and hardenability do not meet the requirements of high-speed train gearbox bearing steel. In order to localize high-speed train bearings, it is necessary to improve the process control level of the vacuum degassing continuous casting process so that the product quality reaches the advanced foreign level, thereby replacing imports. Summary of the invention

[0005] The purpose of the present invention is to provide a high-speed train gearbox bearing steel and a preparation method thereof. By designing a new component of bearing steel, a new carburized bearing steel material different from the steel types listed in the current national standard GB / T 3203 is proposed. By innovating and optimizing the vacuum degassing, continuous casting and rolling processes, the purity and uniformity of the steel are improved, thereby improving the mechanical properties and hardenability of the steel, making the steel more impact-resistant and meeting the quality requirements of high-speed train gearbox bearing steel. At the same time, the product quality reaches the advanced level abroad, and finally realizes the localization of high-speed train gearbox bearing materials to replace imports.

[0006] In order to meet the requirement of high service life of high-speed train gearbox bearings, the steel is required to have high purity. The present invention puts forward strict requirements on microscopic inclusions, macroscopic inclusions and contact fatigue life of steel. Since Class B and Class D inclusions are brittle inclusions with high hardness, they will not deform under the action of stress. Therefore, during the operation of high-speed train gearbox bearings, stress concentration is likely to occur near these brittle inclusions, thereby initiating cracks and causing premature failure of the gearbox bearings. Moreover, the larger the size of such inclusions, the greater the harm. Since Class A and Class C inclusions are plastic inclusions with high ductility, they are less harmful to the service life of the gearbox bearings.

[0007] The present invention requires that microscopic non-metallic inclusions be inspected according to the GB / T 10561-2005A method. The specific requirements for the rating of microscopic non-metallic inclusions are shown in Table 1 below.

[0008] Table 1

[0009]

[0010] The macro defects of the present invention are inspected by the water immersion high frequency flaw detection method according to SEP 1927:2010-08 (water immersion ultrasonic determination method for purity of forged steel bars), using 5-level sensitivity detection, and the total detection volume is ≥5dm 3 , macro inclusions achieve zero defects.

[0011] The steel of the present invention is subjected to contact fatigue life test according to JB / T10510-2005. At room temperature (20°C ± (0-5°C)) and 4.5GPa cyclic stress conditions, the heat treatment quality of the fatigue life specimen block meets the requirements of GB / T8881-2011. The final requirement is that the steel contact fatigue rated life L 10 ≥4×10 7 Second-rate.

[0012] The uniformity and density of the macrostructure of steel affect the life of the bearing. The present invention requires that the macrostructure of the product adopts GB / T 1979-2001 for grading the macrostructure of steel, requiring central porosity ≤1.0 level, general porosity ≤1.0 level, ingot segregation ≤1.0 level, and shrinkage cavities, cracks and subcutaneous bubbles are not allowed.

[0013] The hardenability of the present invention is tested according to GB / T225-2006, and its specific requirements are shown in Table 2 below.

[0014] Table 2

[0015]

[0016] The tensile specimen of the present invention is tested according to GB / T228.1-2010, and the impact specimen is tested according to GB / T229-2007 (the impact specimen adopts a U-shaped notch with a groove depth of 2 mm). The specific testing requirements are shown in Table 3 below.

[0017] Table 3

[0018]

[0019] The technical solution adopted by the present invention to solve the above problems is: a high-speed motor vehicle gearbox bearing steel has the following chemical compositions by mass percentage: C: 0.20-0.25%, Si: 0.35-0.45%, Mn: 0.75-0.95%, Cr: 0.80-0.90%, Mo: 0.25-0.35%, Ni: 1.75-2.05%, Cu: 0.10-0.15%, Nb: 0.06-0.10%, V: 0.08-0.12%, Al≤0.05%, P≤0.015%, S≤0.005%, Ca≤0.0005%, Ti≤0.0015%, O≤0.0008%, H≤0.0002%, As≤0.010%, Sn≤0.010%, Sb≤0.005%, Pb≤0.0015%, and the remainder is Fe and unavoidable impurities.

[0020] The main chemical composition design basis of the steel of the present invention is as follows:

[0021] 1) Determination of C content

[0022] C is one of the most economical and basic elements that affect the strength of steel. At the same time, the C element promotes the formation of austenite during the heating process, and makes the steel obtain high hardness after carburizing heat treatment. Increasing the C content can significantly improve the yield strength and tensile strength of the steel, but it will reduce the plasticity and impact toughness of the steel to a certain extent. According to the use requirements of high-speed train gearbox bearings, the surface of the material must have a higher strength after heat treatment, and the core is also required to have a certain plasticity and impact toughness. Therefore, the C content of the method of the present invention is determined to be 0.20% to 0.25%.

[0023] 2) Determination of Si content

[0024] Adding Si into steel can strengthen ferrite, improve strength, elastic limit and hardenability. The Si content of the present invention is designed to be 0.35% to 0.45%.

[0025] 3) Determination of Mn content

[0026] Mn is a deoxidizing element in the steelmaking process and an effective element for strengthening steel. It plays a role of solid solution strengthening and can improve the hardenability of steel. The Mn content of the present invention is designed to be 0.75% to 0.95%.

[0027] 4) Determination of Cr content

[0028] Cr is an element that improves the hardenability of steel and helps to increase its strength. When the C content is low, adding an appropriate amount of Cr can ensure that the steel reaches the required hardenability and strength; but when the Cr content is too high, it combines with the carbon in the steel to easily form large carbides. Such insoluble carbides reduce the toughness of the steel and shorten the life of the bearing. Therefore, the Cr content of the present invention is designed to be within the range of 0.80% to 0.90%.

[0029] 5) Determination of Cu content

[0030] Cu can improve the hardenability, atmospheric corrosion resistance and seawater corrosion resistance of steel, and reduce the hydrogen-induced crack sensitivity of steel. However, too high Cu content can easily cause cracks on the surface of steel. Therefore, Cu is determined to be 0.10% to 0.15%.

[0031] 6) Determination of Nb and V content

[0032] By adding Nb and V to steel, the CCT curve of the steel can be moved to the lower right, and the stability of austenite can be increased. Most of the Nb and V exist in the steel in the form of carbide, nitride, and carbonitride precipitates. Such precipitates are usually nano-sized. These dispersed small-sized precipitates can pin the austenite grain boundaries, hinder the growth of austenite grains, and refine the austenite grains of the steel. The Nb content of the present invention is designed to be 0.06% to 0.10%, and the V content is designed to be 0.08% to 0.12%.

[0033] 7) Determination of Mo content

[0034] Molybdenum can refine the grains of steel, improve hardenability and heat resistance, and maintain sufficient strength and creep resistance at high temperatures. However, molybdenum is a ferrite-forming element. When the molybdenum content is high, ferrite delta phase or other brittle phases are likely to appear, which reduces toughness. The Mo content of the present invention is determined to be in the range of 0.25% to 0.35%.

[0035] 8) Determination of Ni content

[0036] Ni is an element that improves the hardenability of steel and is also the most commonly used element to effectively improve the wear resistance of steel. The complex effect of Ni with Cr and residual P in steel will help improve the corrosion resistance and wear resistance of steel. Therefore, Ni is determined to be 1.75% to 2.05%.

[0037] 9) Determination of Al content

[0038] Al is added as a deoxidizing element in steel. In addition to reducing the dissolved oxygen in molten steel, Al and N form dispersed and fine aluminum nitride inclusions to refine the grains. However, when the Al content is too high, large particles of Al2O3 and other brittle inclusions are easily formed during the molten steel smelting process, which reduces the purity of the molten steel and affects the service life of the finished product. The present invention requires Al≤0.05%.

[0039] 10) Determination of Ca content

[0040] Ca content will increase the number and size of point oxides in steel. At the same time, due to the high hardness and poor plasticity of point oxides, they do not deform when the steel is deformed, and are prone to form gaps at the interface, which deteriorates the performance of the steel. The present invention requires Ca≤0.0005%.

[0041] 11) Determination of Ti content

[0042] During the solidification of molten steel, Ti is very easy to combine with N or C to form TiN or Ti(C,N) type non-metallic inclusions, which are usually block inclusions with "angular" shapes. Such inclusions have high hardness, seriously affecting the uniformity of the structure, and easily causing stress concentration at the angular parts during operation, seriously reducing the fatigue life of the bearing. Therefore, the present invention requires Ti≤0.0015%.

[0043] 12) Determination of O content

[0044] Oxygen naturally enters the steel during the steelmaking process and remains in the steel at a later stage. Oxygen exists in the steel mainly in the form of non-metallic inclusions such as SiO2 and Al2O3, especially Al2O3 inclusions, which seriously affect the fatigue life of bearings. A large number of fatigue life tests have shown that reducing the oxygen content is significantly beneficial to improving the purity of steel, especially reducing the content and size of oxide brittle inclusions. The present invention requires O≤0.0008%.

[0045] 13) Determination of P and S content

[0046] The P element causes element segregation during the solidification of steel. It dissolves in ferrite to make the grains distorted and coarse, and increases the cold brittleness. Therefore, P is determined to be ≤ 0.015%. The S element easily makes the steel hot brittle, reduces the ductility and toughness of the steel, and the formed sulfides also destroy the continuity of the steel. Therefore, S is determined to be ≤ 0.005%.

[0047] 14) Determination of H content

[0048] H is prone to hydrogen embrittlement in steel, which eventually causes cracks in the steel, thus seriously affecting the service life of the steel. Therefore, H is determined to be ≤ 0.0002%.

[0049] 15) Determination of As, Sn, Sb and Pb contents

[0050] Trace elements such as As, Sn, Sb, and Pb are all low-melting-point nonferrous metals. Their presence in steel causes soft spots on the surface of parts and uneven hardness. Therefore, they are regarded as harmful elements in steel. The content range of these elements in the present invention is determined as As≤0.010%, Sn≤0.010%, Sb≤0.005%, and Pb≤0.0015%.

[0051] The present invention discloses a production method for high-speed train gearbox bearing steel, and the process flow is KR (molten iron pretreatment) → converter or electric furnace → ladle refining furnace LF furnace → vacuum circulating degassing furnace RH or VD furnace → continuous casting CCM (large cross section) → slow cooling → heating and rolling into material → finishing → surface and internal flaw detection → packaging.

[0052] The main steps are as follows:

[0053] (1) Molten steel smelting:

[0054] KR (hot metal pretreatment), converter or electric furnace: hot metal pretreatment is carried out in KR, CaO-FeO composite powder is blown into the hot metal tank using nitrogen and oxygen composite gas as a carrier for dephosphorization, desulfurization and detitanium treatment, and chemical reactions are carried out under mechanical stirring to dephosphorize (P≤0.075%), desulfurize (S≤0.008%), and detitanium (Ti≤0.0040%), and then the harmful slag obtained by the reaction is removed by a mechanical arm to ensure the cleanliness of the hot metal; secondly, primary smelting is carried out in a converter or electric furnace, oxygen is blown into the top of the furnace mouth for oxidation reaction, and argon is blown into the bottom for stirring. Preferably, the oxygen blowing amount per ton of steel is 30 cubic meters to 40 cubic meters, and the argon gas amount per ton of steel is 0.5 cubic meters to 1 cubic meter. Active slag-forming agent (CaO-CaF2) is added to further remove harmful elements of phosphorus (P≤0.010%) and titanium (Ti≤0.0015%) under the comprehensive action of oxygen and argon, and the terminal carbon of the primary furnace is controlled to be 0.08%-0.12% when tapping steel, and the tapping temperature is ≥1640°C. Slag blocking is adopted for tapping steel. During the tapping process, Al wire (100Kg-150Kg) is first fed for precipitation deoxidation, and then the main elements required in the steel are added: C is adjusted to 0.15%-0.20%, Si is adjusted to 0.35%-0.40%, Mn is adjusted to 0.75%-0.85%, Cr is adjusted to 0.70%-0.80%, Cu is adjusted to 0.10%-0.15%, Ni is adjusted to 1.75%-2.05%, and Mo is adjusted to 0.25%-0.35%. After the molten steel is exhausted, it is quickly hoisted to the refining LF furnace for smelting;

[0055] Refining furnace: The whole refining process adopts bottom blowing argon to stir the molten steel, and slag is formed on the surface of the molten steel. During the process, Al wire and CaO-SiC high-performance composite slag-making agent are used for deoxidation and removal of harmful non-metallic inclusions. The aluminum wire enters deep into the molten steel for precipitation deoxidation, and the CaO-SiC high-performance composite slag-making agent diffuses on the surface of the molten steel for deoxidation and adsorbs and removes harmful non-metallic inclusions. During the smelting process, firstly, Al wire (100 kg) is fed into the molten steel, and then CaO-SiC high-performance composite slag-making agent (600 kg) is added at one time, argon gas is connected to the bottom of the ladle, and then the electrode is inserted into the slag for submerged arc power-on. After 10 minutes of power-on, the molten steel is temperature-measured and sampled for analysis. According to the sampling results, the required main elements (V, Nb, etc.) are added according to the target requirements through computer software. The number of temperature measurement and sampling of the refining furnace is controlled at 2-3 times, and the whole refining process time is controlled at ≥50 minutes; while adjusting the content of the required main elements, the purpose of deoxidation and removal of non-metallic inclusions is achieved. No alloy is allowed to be added within 15 minutes before the end of refining. Finally, the power is stopped, and the argon gas flow at the bottom of the ladle is reduced until the molten steel is not exposed to the air. The soft blowing time of the molten steel is 10 minutes to 15 minutes, so that harmful inclusions can be fully floated and removed;

[0056] Vacuum degassing: During RH or VD vacuum degassing, the maximum vacuum degree in the vacuum furnace is ≤1.33mbar, and the vacuum cycle treatment time of molten steel is maintained for ≥25min to ensure that the harmful gas hydrogen in the steel is effectively removed. After the vacuum treatment is completed, argon is blown into the bottom of the ladle, and the argon flow rate is controlled so that the molten steel is not exposed to the air. The soft blowing time of the molten steel is 10min to 15min. Finally, the harmful gases and non-metallic inclusions in the steel are further removed;

[0057] (2) Continuous casting: argon protection is used throughout the casting process to prevent secondary contamination and oxidation of the molten steel; preferably, low superheat casting is used (superheat △T≤20°C); the amount of molten steel in the tundish is controlled at 30-35 tons, and the light pressure control technology (pressure reduction 15mm-20mm) is used, and the casting speed is 0.5-0.55m / min; an appropriate steel flow to water ratio (0.75-0.95L / kg) is used; electromagnetic stirring is used in the tundish to interrupt the bridging of the columnar crystal zone during the solidification of the continuous casting billet; through the above various control technologies, the surface and internal quality of the molten steel are further improved;

[0058] (3) Slow cooling of continuous casting billets: Preferably, the continuous casting billets are quickly lifted off the production line and then slowly cooled in a slow cooling pit. The slow cooling temperature of the continuous casting billets off the production line is ≥600°C, and the billets are covered with a heat preservation cover. The slow cooling time is ≥48 hours, and the pit temperature is ≤200°C.

[0059] (4) Heating and rolling: The continuous casting billet is transferred to a heating furnace with a neutral or weakly oxidizing atmosphere for heating and then rolled into round bars. The specific rolling process is as follows: the continuous casting billet is first hoisted to the conveyor roller, and then enters the walking-beam heating furnace through the conveyor roller. The steel is heated to 1150℃~1200℃ in the heating furnace, and the insulation time is 4h~5h. The temperature of the continuous casting billet after being discharged from the furnace is 1050℃~1100℃. The continuous casting billet is conveyed to the high-pressure water descaling through the roller. On the one hand, descaling removes the oxidized iron scale on the surface of the continuous casting billet, and on the other hand, it quickly reduces the surface temperature of the continuous casting billet. When the surface temperature of the billet is 100-200℃ lower than the core temperature, 4-pass reciprocating turning large reduction technology is adopted (the steel is turned 90° after each pass), and the four-pass reduction amounts are 25%~30%, 15%~20%, 20%~25%, and 25%~30% respectively, so that the core structure of the billet is deformed and recrystallized preferentially during the deformation process, so that the central structure of the steel is more uniform and dense under the action of large pressure. Then it is rolled alternately by 4 horizontal and vertical rolling mills, and finally the round bars with specifications of Φ130mm~Φ200mm are rolled and slowly cooled off the line;

[0060] (5) Finishing: including straightening, chamfering and other finishing processes to ensure that indicators such as size and curvature meet the requirements.

[0061] (6) The surface and interior are subjected to 100% non-destructive testing, and only those that pass the inspection can be considered qualified products.

[0062] Compared with the prior art, the advantages / features of the present invention are:

[0063] 1. From the perspective of manufacturing technology, the production process of vacuum degassing and continuous casting greatly shortens the production cycle, improves the yield rate and production efficiency, realizes large-scale production, and is conducive to improving the stability of material composition and product quality compared to the die casting technology.

[0064] 2. From the perspective of composition design, in order to improve the plasticity and toughness of steel, the present invention relates to a new type of carburized bearing steel material that is different from the steel types listed in the current national standard GB / T 3203, which meets the requirements for high-speed train gearbox bearing steel.

[0065] 3. Special smelting process:

[0066] (1) KR (hot iron pretreatment): Nitrogen-oxygen composite gas is used as a carrier to inject CaO-FeO composite powder for dephosphorization, desulfurization and detitanium treatment.

[0067] (2) Converter or electric furnace: Add active slag-forming agent (CaO-CaF2) under the combined action of oxygen and argon to further remove harmful elements such as phosphorus and titanium. When tapping steel, feed Al wire for precipitation deoxidation and add certain main elements.

[0068] (3) Refining furnace and vacuum degassing furnace: In the LF refining furnace, Al wire and CaO-SiC high-performance composite slag-making agent are used for deoxidation and removal of harmful non-metallic inclusions. In the RH or VD vacuum degassing furnace, the hydrogen content in the steel is further removed in a vacuum environment, ultimately reducing the non-metallic inclusions and O and H contents in the steel to extremely low levels, with the number and size of inclusions reaching the world's leading level.

[0069] (4) Continuous casting uses argon protection throughout the pouring process to protect the molten steel from secondary oxidation contamination; low superheat pouring (superheat △T ≤ 20℃), light pressure control technology (pressure reduction 15mm~20mm), appropriate steel flow water ratio (0.75~0.95L / kg) and tundish electromagnetic induction technology to ensure that the steel has good surface and internal quality.

[0070] (5) The continuous casting billet is lifted and quickly taken off the production line for slow cooling in the slow cooling pit. The slow cooling temperature of the continuous casting billet off the production line is ≥600℃, and the insulation cover is covered. The slow cooling time is ≥48 hours, and the pit temperature is ≤200℃.

[0071] 4. Through four-pass high-pressure rolling technology (the steel is turned 90° after each pass), the four-pass reduction amounts are 25%-30%, 15%-20%, 20%-25%, and 25%-30% respectively, so that the core structure of the ingot is deformed and recrystallized preferentially during the deformation process, so that the central structure of the steel is more uniform and dense under the action of high pressure, further improving the uniformity of the steel structure.

[0072] 5. The high-speed train gearbox bearing steel produced by the present invention meets the following index requirements:

[0073] Microscopic inclusions are inspected according to GB / T 10561A method. Non-metallic inclusions meet the requirements of Class A fine system ≤1.5; Class A coarse system ≤1.0; Class B fine system ≤1.0; Class B coarse system ≤0.5; Class C fine system = 0; Class C coarse system = 0; Class D fine system ≤0.5; Class D coarse system ≤0.5; Ds class ≤0.5. Macroscopic defects are inspected according to SEP 1927 water immersion high frequency flaw detection method, using 5-level sensitivity detection, and the total detection volume ≥5dm 3 , the macro inclusions reach zero defects; the contact fatigue life test is carried out according to JB / T10510-2005. At room temperature (20℃±5℃) and 4.5GPa cyclic stress conditions, the heat treatment quality of the fatigue life specimen block meets the requirements of GB / T8881-2011, requiring the steel contact fatigue rated life L 10 ≥4×10 7 times; the macrostructure adopts GB / T 1979-2001 to grade the macrostructure of steel, requiring central porosity ≤1.0, general porosity ≤1.0, ingot segregation ≤1.0, and shrinkage, cracks and subcutaneous bubbles are not allowed; hardenability is tested according to GB / T225-2006, J1.5 = 45 ~ 50HRC, J9 = 36 ~ 45HRC; tensile strength is tested according to GB / T228.1-2010, impact is tested according to GB / T229-2007, tensile strength (R m )≥1200MPa, elongation (A)≥18%, section shrinkage (Z)≥55%, impact absorption energy (KU2)≥130J. DETAILED DESCRIPTION

[0074] The present invention is further described in detail below in conjunction with examples. The examples are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0075] The manufacturing process of the steel for high-speed train bearing rolling elements in the embodiment of the present invention is to adopt KR (molten iron pretreatment) → converter or electric furnace → ladle refining furnace LF furnace → vacuum circulation degassing furnace RH or VD furnace → continuous casting CCM (large cross-section) → slow cooling → hot rolling into materials → finishing → surface and internal flaw detection → packaging.

[0076] Specifically, in KR, CaO-FeO composite powder is injected into the molten iron tank with nitrogen-oxygen composite gas as a carrier for dephosphorization, desulfurization and detitanium treatment, and then the harmful slag obtained by the reaction is removed by a mechanical arm. For the treated molten iron, P≤0.075%, S≤0.008%, and Ti≤0.0040% in the three embodiments; in the production process of the electric furnace / converter, the oxygen blowing amount per ton of steel is 32 / 34 / 35 cubic meters, the argon gas amount per ton of steel is 0.55 / 0.6 / 0.63 cubic meters, the end point C of steel tapping is controlled at 0.08% to 0.12%, the end point P is controlled at ≤0.010%, the end point Ti≤0.0015%, the tapping temperature is controlled at 1645℃ to 1660℃, and the slag blocking system is used to block the slag during the tapping process. Al wire (100Kg to 1 50Kg) is used for precipitation deoxidation, and then the main elements required in the steel are added, C is added to 0.15%-0.20%, Si is added to 0.35%-0.40%, Mn is added to 0.75%-0.85%, Cr is added to 0.70%-0.80%, Cu is added to 0.10%-0.15%, Ni is added to 1.75%-2.05%, and Mo is added to 0.25%-0.35%. After the molten steel is exhausted, it is quickly hoisted to the refining LF furnace; in the LF refining furnace, Al wire (100Kg) is first fed into the molten steel, and then CaO-SiC high 600Kg of high-performance composite slag-making agent was added. Argon was connected to the bottom of the ladle, and then the electrode was inserted into the slag for submerged arc power-on. After 10 minutes of power-on, the molten steel was temperature-measured and sampled for analysis. According to the sampling results, the required main elements (V, Nb, etc.) were added according to the target requirements through computer software. The number of temperature measurement and sampling in the refining furnace was controlled at 2-3 times. The whole refining process took 50-60 minutes. While adjusting the content of the required main elements, the purpose of deoxidation and removal of non-metallic inclusions was achieved. No alloy was added within 15 minutes before the end of refining. Finally, the power was stopped and the argon flow at the bottom of the ladle was reduced. The molten steel is not exposed to the air, and the soft blowing time of the molten steel is 10min~15min, so that harmful inclusions can be fully floated and removed; during RH or VD vacuum degassing, the maximum vacuum degree in the vacuum furnace is ≤1.33mbar, the vacuum circulation treatment time of the molten steel is ≥25min, and the soft blowing time of the molten steel is 10min~15min; the continuous casting overheat is controlled within ≤20℃, the continuous casting speed is controlled at 0.5~0.55m / min, the light pressure reduction is 15mm~20mm, the molten steel volume in the tundish is controlled at 30~35 tons, and the steel flow to water ratio is controlled at 0.75~0.95L / kg; the continuous casting billet is lifted and quickly taken off the line for slow cooling in the slow cooling pit. The slow cooling temperature of the continuous casting billet off the line is ≥600℃, covered with an insulation cover, the slow cooling time is ≥48 hours, and the pit opening temperature is ≤200℃; the continuous casting billet taken out of the pit is first lifted to the conveyor roller, and then enters the walking beam heating furnace with a neutral or weak oxidizing atmosphere through the conveyor roller. The steel is heated to 1150℃~1200℃ in the heating furnace, and the insulation time is 4h~5h. The temperature of the continuous casting billet after leaving the furnace is 1050℃~1100℃, the continuous casting billet is conveyed to high-pressure water for descaling through rollers, and then a 4-pass reciprocating turning large reduction technology is adopted (the steel is turned 90° after each pass), and the four-pass reduction amounts are 25%~30%, 15%~20%, 20%~25%, and 25%~30%, respectively, and then it is rolled alternately through 4 horizontal and vertical rolling mills, and finally the round bars with specifications of Φ130mm~Φ200mm are rolled, and then slowly cooled to room temperature off the line. Then the bars are subjected to subsequent flaw detection and finishing. .

[0077] The chemical composition (wt%) of the steel for high-speed train gearbox bearings of various embodiments of the present invention and that of imported materials (for comparison) are shown in Tables 4 and 5.

[0078] Table 4

[0079]

[0080]

[0081] Table 5

[0082] Mo As Sn Sb Pb Nb V Ti O Embodiment 1 of the present invention 0.30 0.0041 0.0012 0.0011 0.0010 0.08 0.05 0.0007 0.00047 Embodiment 2 of the present invention 0.29 0.0048 0.0010 0.0015 0.0010 0.07 0.05 0.0007 0.00042 Embodiment 3 of the present invention 0.30 0.0045 0.0011 0.0014 0.0010 0.08 0.06 0.0008 0.00044 Contrast steel 0.24 0.0082 0.0032 0.0035 0.0010 0.001 0.001 0.0022 0.00083

[0083] From the composition point of view, the imported material belongs to the G20CrNi2Mo carburized bearing steel listed in GB / T 3203, while the present invention is a new type of carburized bearing steel different from the current steel types listed in GB / T 3203, and Cu, V and Nb elements are added; in addition, compared with imported materials, the present invention has obvious advantages in controlling the content of harmful elements such as oxygen, titanium, phosphorus and sulfur.

[0084] Table 6 Inclusions in the steel materials of each example

[0085]

[0086] From the detection of non-metallic inclusions, the material of the present invention is slightly better than that of imported materials.

[0087] Table 7 Low-power data of steel materials in various examples

[0088]

[0089] From the low-magnification test results, the material of the present invention is slightly better than the imported material.

[0090] Table 8 Water immersion high frequency flaw detection data of steel materials in various embodiments

[0091]

[0092]

[0093] From the water immersion high frequency flaw detection, the invention did not find any macroscopic inclusion defects, while the imported material had macroscopic defects with a length of 3 mm.

[0094] Table 9 Contact fatigue life data of steel materials in various embodiments

[0095]

[0096] From the contact fatigue life test data, the rated life L 10 All greater than 4.0×10 7 Second, better than imported materials.

[0097] Table 10 End hardenability data of steel materials in various examples

[0098]

[0099] From the end hardenability test data, the end hardenability of the material of the present invention is better than that of imported materials.

[0100] Table 11 Mechanical properties data of steel materials in various embodiments

[0101]

[0102] From the end hardenability test data, it can be seen that the mechanical properties of the present invention are obviously greatly improved and are better than imported materials.

[0103] From the comparison of Tables 4, 5, 6, 7, 8, 9, 10 and 11, it can be seen that the high-speed train gearbox bearing steel in each embodiment of the present invention has the following differences and advantages compared with the imported steel:

[0104] 1. The main chemical composition design is different. In order to meet the requirements of high-speed train gearbox bearing steel, the steel composition is specially designed, which greatly improves the mechanical properties and end hardenability of the steel. The result is significantly better than imported steel.

[0105] 2. The present invention adopts KR spraying CaO-FeO composite powder dephosphorization, desulfurization and detitanium technology; the converter or electric furnace adopts a new slag-making agent (CaO-CaF2) under the comprehensive action of appropriate oxygen and argon to further remove harmful elements of phosphorus and titanium; the refining LF furnace uses Al wire and CaO-SiC high-performance composite slag-making agent to deoxidize and remove harmful non-metallic inclusions, and the vacuum degassing RH / VD furnace further removes hydrogen in the steel under vacuum conditions; the continuous casting adopts full-process argon protection pouring, low superheat pouring, tundish electromagnetic induction and other control technologies, which ultimately makes the harmful elements, non-metallic inclusions and water immersion high-frequency flaw detection results of molten steel significantly better than those of imported steel.

[0106] 3. From the low-power inspection results, since the continuous casting of the present invention adopts the light reduction technology and combines the 4-pass large reduction rolling technology, in addition, a small amount of alloy elements Nb and V are added in the smelting process. By adding Nb and V to the steel, the CCT curve of the steel can be moved to the lower right, the stability of austenite can be increased, the austenite grain boundary can be pinned, the growth of austenite grains can be hindered, and the austenite grains of the steel can be refined, so that the low-power quality of the steel is better than that of imported materials.

[0107] 4. From the contact fatigue life results, the present invention adopts a special smelting method in the process of smelting carburized steel to improve the contact fatigue life. At the same time, the present invention also adds some V and Cu elements that improve the toughness, wear resistance and corrosion resistance of the steel to further improve the contact fatigue life of the steel, so that the contact fatigue rated life L of the present invention is 10 Greater than 4.0×10 7 It is better than imported materials.

[0108] In summary, the present invention adopts a continuous casting process to produce high-speed EMU gearbox bearing steel and a production method thereof. Through a new design of the chemical composition of the steel, a high-efficiency, high-capacity, and low-cost process route of vacuum degassing, continuous casting, and rolling is adopted, and a special control method is used in each key process. Finally, a new process for producing high-speed EMU gearbox bearing steel by vacuum degassing + continuous casting is formed, thereby obtaining steel with high purity, high homogeneity, high mechanical properties and high fatigue life. The steel is more competitive in production efficiency, production cost, and product quality stability, and finally replaces imported materials.

[0109] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.

Claims

1. A steel for high-speed train gearbox bearings, characterized in that: The chemical composition of the steel meets the following requirements by mass percentage: C: 0.20-0.25%, Si: 0.35-0.45%, Mn: 0.75-0.95%, Cr: 0.80-0.90%, Mo: 0.25-0.35%, Ni: 1.75-2.05%, Cu: 0.10-0.15%, Nb: 0.06-0.10%, V: 0.08-0.12%, Al≤0.05%, P≤0.015%, S≤0.005%, Ca≤0.0005%, Ti≤0.0015%, O≤0.0008%, H≤0.0002%, As≤0.010%, Sn≤0.010%, Sb≤0.005%, Pb≤0.0015%, and the balance is Fe and unavoidable impurities; The contact fatigue life test was carried out in accordance with JB / T10510-2005. At room temperature: 20℃±5℃ and 4.5GPa cyclic stress conditions, the heat treatment quality of the fatigue life specimen block met the requirements of GB / T8881-2011, requiring the steel contact fatigue rated life L 10 ≥4×10 7 times; hardenability is tested according to GB / T225-2006, J1.5=45~50HRC, J9=36~45HRC; tensile strength is tested according to GB / T228.1-2010, impact strength is tested according to GB / T229-2007, tensile strength R m ≥1200MPa, elongation A≥18%, section shrinkage Z≥55%, impact absorption energy KU2≥130J.

2. The high-speed train gearbox bearing steel according to claim 1, characterized in that: Microscopic non-metallic inclusions are inspected according to GB / T10561-2005A method, and the rating of microscopic non-metallic inclusions meets the following requirements: 。 3. The high-speed train gearbox bearing steel according to claim 1, characterized in that: According to SEP 1927:2010-08 forging steel bar purity water immersion ultrasonic determination method to detect macro defects, using 5-level sensitivity detection, the total detection volume ≥ 5dm 3 , macro inclusions achieve zero defects.

4. The high-speed train gearbox bearing steel according to claim 1, characterized in that: According to GB / T1979-2001, the macrostructure of steel is graded as follows: central porosity ≤1.0, general porosity ≤1.0, ingot segregation ≤1.0, and there are no shrinkage cavities, cracks or subcutaneous bubbles.

5. A method for manufacturing the high-speed train gearbox bearing steel according to claim 1, characterized in that: The steps include: (1) Molten steel smelting: KR hot metal pretreatment, converter or electric furnace: Hot metal pretreatment is carried out in KR, and CaO-FeO composite powder is sprayed into the hot metal tank with nitrogen and oxygen composite gas as a carrier for dephosphorization, desulfurization and detitanium treatment. Under the action of mechanical stirring, chemical reaction is carried out to dephosphorize P≤0.075%, desulfurize S≤0.008%, and detitanium Ti≤0.0040%, and then the harmful slag obtained by the reaction is removed; secondly, primary refining is carried out in a converter or electric furnace, oxygen is blown into the top of the furnace mouth to oxidize the molten steel, argon is blown into the bottom for stirring, and active slag-making agent is added to further remove harmful elements phosphorus: P≤0.010% and titanium: T under the combined action of oxygen and argon. i≤0.0015%, control the final carbon of the primary furnace when tapping: 0.08%~0.12%, tapping temperature ≥1640℃, tapping with slag blocking, first feed Al wire for precipitation deoxidation during tapping, then add the main elements required in the steel, adjust C to 0.15%~0.20%, Si to 0.35%~0.40%, Mn to 0.75%~0.85%, Cr to 0.70%~0.80%, Cu to 0.10%~0.15%, Ni to 1.75%~2.05%, Mo to 0.25%~0.35%, after the molten steel is exhausted, quickly lift it to the refining LF furnace for smelting; Refining furnace: The whole refining process uses bottom blowing argon to stir the molten steel, and slag is formed on the surface of the molten steel. During the process, Al wire and CaO-SiC high-performance composite slag-making agent are used for deoxidation and removal of harmful non-metallic inclusions. The aluminum wire enters the deep part of the molten steel for precipitation deoxidation, and the CaO-SiC high-performance composite slag-making agent diffuses deoxidation on the surface of the molten steel and adsorbs and removes harmful non-metallic inclusions. During the smelting process, Al wire is first fed into the molten steel, and then the CaO-SiC high-performance composite slag-making agent is added. The bottom of the ladle is connected to argon gas, and then the electrode is inserted into the slag for submerged arc power-on. After 10 minutes of power-on, , measure the temperature of the molten steel and take samples for analysis. According to the sampling results, add the required main elements according to the target requirements through computer software. The number of temperature measurement and sampling of the refining furnace is controlled at 2-3 times, and the whole refining process time is controlled at ≥50min; while adjusting the content of the required main elements, the purpose of deoxidation and removal of non-metallic inclusions is achieved. No alloy is allowed to be added within 15 minutes before the end of refining. Finally, stop the power supply, adjust the argon flow at the bottom of the ladle until the molten steel is not exposed to the air, and the soft blowing time of the molten steel is 10min~15min, so that harmful inclusions can be fully floated and removed; Vacuum degassing: During RH or VD vacuum degassing, the maximum vacuum degree in the vacuum furnace is ≤1.33mbar, and the vacuum cycle treatment time of molten steel is maintained for ≥25min to ensure that the harmful gas hydrogen in the steel is effectively removed. After the vacuum treatment is completed, argon is blown into the bottom of the ladle, and the argon flow rate is controlled so that the molten steel is not exposed to the air. The soft blowing time is 10min~15min; (2) Continuous casting: Use inert gas protection and low superheat casting throughout the entire process; use light pressure control technology; use appropriate steel flow to water ratio; use electromagnetic stirring in the tundish to interrupt the bridging of columnar crystal areas during the solidification of the continuous casting billet; (3) Slow cooling of continuous casting billet; (4) Heating and rolling: The continuous casting billet is heated to 1150℃~1200℃, and the holding time is 4h~5h. The temperature of the continuous casting billet after being taken out of the furnace is 1050℃~1100℃. The continuous casting billet is descaled by high-pressure water. When the surface temperature of the billet is 100-200℃ lower than the core temperature by descaling, a 4-pass reciprocating turning large reduction technology is adopted. After each pass of pressing, the steel is turned 90°. The reduction amounts of the four passes are 25%~30%, 15%~20%, 20%~25%, and 25%~30% respectively. Then, it is rolled alternately by 4 horizontal and vertical rolling mills. Finally, the round bars with specifications of Φ130mm~Φ200mm are rolled and slowly cooled off the line. (5) Finishing.

6. The method according to claim 5, characterized in that: In step (1), the amount of oxygen blown per ton of steel during the primary smelting process is 30 cubic meters to 40 cubic meters, and the amount of argon gas per ton of steel is 0.5 cubic meters to 1 cubic meter; the active slag-forming agent is CaO-CaF2, and the amount of Al wire added during the steelmaking process is 100 kg to 150 kg.

7. The method according to claim 5, characterized in that: In step (1), during the smelting process in the refining furnace, 100 kg of Al wire is first fed into the molten steel, and then 600 kg of CaO-SiC high-performance composite slag-making agent is added at one time.

8. The method according to claim 5, characterized in that: In step (2), the superheat degree △T of molten steel pouring is ≤20°C, the amount of molten steel in the tundish is controlled at 30-35 tons, the pouring and pulling speed is 0.5-0.55 m / min, the reduction amount under light pressure is 15 mm-20 mm, and the steel flow water content is 0.75-0.95 L / kg.

9. The method according to claim 5, characterized in that: In step (3), the continuous casting billet is slowly cooled in a slow cooling pit, the slow cooling temperature of the continuous casting billet is ≥600°C, the billet is covered with an insulation cover, the slow cooling time is ≥48 hours, and the pit start temperature is ≤200°C.

Citation Information

Patent Citations

  • Carburizing bearing steel for railway freight car and preparing method of carburizing bearing steel

    CN107904498A

  • New energy automobile gearbox bearing steel material and manufacturing method thereof

    CN114807759A

  • Steel for bearing rolling body of high-speed motor car and manufacturing method of steel

    CN115369333A

  • Steel material for bearing raceway and bearing raceway

    JP2021127504A