Preparation method and application of copper-doped lanthanum hydroxide nanomaterial
By using copper-doped lanthanum hydroxide nanomaterials as hole transport layers in perovskite solar cells, the problems of poor stability of organic materials and insufficient low-temperature crystallinity of inorganic metal oxides in the existing technology are solved, improving the performance of perovskites. The photoelectric conversion efficiency and stability of solar cells expand their application prospects.
Patent Information
- Application Number
- CN202310478197.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The organic hole transport materials used in existing perovskite solar cells have poor stability and high cost, and the inorganic metal oxides have insufficient crystallinity at low temperatures, which limits the photoelectric conversion efficiency and commercial application of perovskite solar cells.
Copper-doped lanthanum hydroxide nanomaterials are used as the hole transport layer, prepared by hydrothermal method and applied in perovskite solar cells, which expands the selection range of hole transport materials and improves photoelectric conversion efficiency and stability.
Perovskite solar cells based on inorganic metal hydroxides have been achieved with excellent performance, good stability and repeatability, and low cost, expanding the application prospects of perovskite solar cells.
Smart Images

Figure CN116495767B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano material preparation, and specifically relates to a method for synthesizing an inorganic metal hydroxide nano material and applying the method to a perovskite solar cell. Background Art
[0002] In recent years, perovskite solar cells have attracted widespread attention due to their low cost, simple manufacturing process, high photoelectric conversion efficiency, and the ability to be prepared into flexible, transparent and stacked cells. Perovskite solar cells can be divided into two types of structures according to the structural design of the device, namely, the upright structure and the inverted structure. The upright perovskite solar cell is a nip-type structure, specifically, an electron transport layer, a perovskite layer, a hole transport layer, and a metal electrode layer are deposited on the conductive glass in sequence. The inverted perovskite solar cell is a pin-type structure, specifically, a hole transport layer, a perovskite layer, an electron transport layer, and a metal electrode layer are deposited on the conductive glass in sequence. At present, the photoelectric conversion efficiency of the inverted perovskite solar cell is lower than that of the upright perovskite solar cell, but the inverted perovskite solar cell has unique advantages, such as lower hysteresis, good stability, and broad application prospects in tandem solar cells.
[0003] The hole transport layer is indispensable in perovskite solar cells. It plays the role of blocking electrons and conducting holes, which significantly affects the performance of perovskite solar cells. At present, the hole transport materials used in most perovskite solar cells are mainly organic, such as Spiro-OMeTAD and PEDOT:PSS. Spiro-OMeTAD is often used in perovskite solar cells with an upright structure. Due to the poor hole transport ability of Spiro-OMeTAD, Li-TFSI and 4-tert-butylpyridine are often used as additives in Spiro-OMeTAD to improve its hole transport ability. However, such additives are easy to destroy the perovskite layer under high temperature and high humidity conditions. PEDOT:PSS is often used in perovskite solar cells with an inverted structure. It has the characteristics of hygroscopicity and acidity. On the one hand, the hygroscopicity of PEDOT:PSS causes it to absorb moisture from the air, thereby causing the decomposition of the perovskite layer. On the other hand, the acidity of PEDOT:PSS will corrode the conductive glass electrode. Therefore, perovskite solar cells based on organic hole transport materials generally have poor stability. In addition, organic hole transport materials have the disadvantages of complex manufacturing and purification processes and high prices, which hinder the commercial application and promotion of perovskite solar cells.
[0004] In order to solve this problem, researchers have tried to use inorganic hole transport materials with simple manufacturing, low cost and good stability in perovskite solar cells. The hole transport layer of the perovskite solar cell with an upright structure is deposited on top of the perovskite layer, and the perovskite layer is not resistant to polar solvents, high temperature and high humidity. Many nanoparticles of inorganic hole transport materials often need to be dispersed in polar solvents, which makes it difficult to spin-coat the inorganic hole transport materials directly on top of the perovskite layer. In the perovskite solar cell with an inverted structure, the hole transport layer is spin-coated directly on top of the conductive glass, and the polar solvent is evaporated by annealing before the perovskite layer is spin-coated, which avoids contact between the polar solvent and the perovskite layer. Therefore, inorganic hole transport materials are often used in perovskite solar cells with an inverted structure. At present, the common inorganic hole transport materials in perovskite solar cells with an inverted structure are mainly metal oxides, and the common ones are: NiO X 、CoO X , CuO X 、CuGaO 2 etc.
[0005] In addition to inorganic metal oxides, inorganic metal hydroxides also have the characteristics of simple manufacturing process, low cost, good stability, and inorganic metal hydroxides generally have better low-temperature crystallinity than inorganic metal oxides. However, in the field of perovskite solar cells, most of the research on inorganic metal hydroxides is mainly focused on the role of device interface passivation, and there is still little research on inorganic metal hydroxides as carrier transport materials. At present, researchers have synthesized Nb(OH) 5 , and it has been successfully applied as an electron transport material in perovskite solar cells, but its photoelectric conversion efficiency is still relatively low. Therefore, further development of perovskite solar cells based on inorganic metal hydroxides with higher photoelectric conversion efficiency and more stable performance will help promote the commercial development of perovskite solar cells. Summary of the invention
[0006] In order to overcome the shortcomings of the prior art, the present invention provides a novel inorganic metal hydroxide nanomaterial (copper-doped lanthanum hydroxide nanomaterial), and applies it as a hole transport material to perovskite solar cells, so that the perovskite solar cells based on inorganic metal hydroxide hole transport materials obtain good photoelectric conversion efficiency. In addition, the present invention applies inorganic metal hydroxide as a hole transport material to perovskite solar cells for the first time, expanding the selection range of hole transport materials for perovskite solar cells.
[0007] The first object of the present invention is to provide a method for preparing a copper-doped lanthanum hydroxide nanomaterial. The second object of the present invention is to apply the copper-doped lanthanum hydroxide nanomaterial as a hole transport layer in a perovskite solar cell.
[0008] The technical solution adopted by the present invention is as follows:
[0009] A method for preparing a copper-doped lanthanum hydroxide nanomaterial comprises the following steps:
[0010] 1) Prepare a 50 mg / mL polyether P123 solution with deionized water;
[0011] 2) Mix the lanthanum source material and the copper source material into a beaker, wherein the molar amount of copper in the material is 10-40% of the lanthanum, add the polyether P123 solution prepared in step 1), and stir to form a uniform mixed solution; wherein, for every 1 mmol La 3+ Use 3.125 mL of polyether P123 solution;
[0012] 3) Slowly add ethylene glycol to the solution obtained in step 2) and continue stirring to form a uniform mixed solution; wherein, for every 1 mmol La 3+ Use 2.734 mL of ethylene glycol;
[0013] 4) Prepare a 0.5 M potassium hydroxide solution with deionized water;
[0014] 5) Under stirring conditions, slowly add the prepared potassium hydroxide solution to the solution obtained in step 3), and stir to form a uniform mixed solution; wherein, for every 1 mmol La 3+ Use 6.25mL of potassium hydroxide solution;
[0015] 6) transferring the solution obtained in step 5) to a reaction kettle and heating at 210 degrees Celsius for 50 minutes;
[0016] 7) After the hydrothermal reaction in step 6) is completed and the reactor is cooled, the supernatant is removed by centrifugation to obtain a crude product, and the reaction product is then washed with dilute ammonia water and isopropanol in sequence to finally obtain a copper-doped lanthanum hydroxide nanomaterial.
[0017] Furthermore, the lanthanum source material and the copper source material in step 2) can be selected from nitrates or sulfates, preferably lanthanum nitrate and copper nitrate, and the molar amount of copper nitrate is 10% to 40% of the lanthanum nitrate, preferably 25%.
[0018] An application of a copper-doped lanthanum hydroxide nanomaterial is to apply the copper-doped lanthanum hydroxide nanomaterial as a hole transport layer to a perovskite solar cell, comprising the following steps:
[0019] 1) The etched 1.5 cm×1.5 cm fluorine-doped tin dioxide conductive glass substrate was ultrasonically cleaned in isopropanol, deionized water, and ethanol for 15 min, and then treated with ultraviolet ozone for 15 min;
[0020] 2) The copper-doped lanthanum hydroxide nanomaterial synthesized above was dispersed in a mixed solvent of dimethyl sulfoxide and isopropanol with a volume ratio of 1:1 using a cell crusher, and then spin-coated on a transparent conductive glass substrate, with the spin coating parameters set to 7000r / m, 50s, and after the spin coating, annealed on a heating plate at 100°C for 10min, and the spin coating and annealing process was repeated four times to obtain a hole transport layer;
[0021] 3) methylamine bromide, lead bromide, cesium iodide, iodomethane and lead iodide are mixed in a molar ratio of 1:1.9:2.3:10:11.4, and then dissolved in a mixed solvent of dimethylformamide and dimethyl sulfoxide in a volume ratio of 4:1, using 9.2 mL of the mixed solvent for every 1 mmol of methylamine bromide, and finally adding 1% of the total volume of the mixed solvent hydroxyethyl acrylate, and mixing well to obtain a perovskite precursor solution;
[0022] 4) Spin coating the perovskite precursor solution on the hole transport layer by a two-step spin coating method, with the parameters set as follows: the first step of spin coating is 500 r / m, 5 s, and the second step of spin coating is 5000 r / m, 45 s; 30 s before the end of spin coating, 100 uL of chlorobenzene anti-solvent is added dropwise, and after the spin coating is completed, annealing is performed on a 100° C. hot plate for 10 min to obtain a perovskite layer;
[0023] 5) preparing a 1 mg / mL phenethylammonium iodide solution using isopropanol as the solvent;
[0024] 6) Spin-coat the phenylethyl ammonium iodide solution on the perovskite layer at a speed of 4000 r / m for 30 seconds. After the spin-coating, anneal on a hot plate at 100° C. for 10 minutes to obtain an interface passivation layer;
[0025] 7) preparing a 20 mg / mL solution of [6,6]-phenyl C61 butyric acid methyl ester using chlorobenzene as solvent;
[0026] 8) Spin-coating the [6,6]-phenyl C61 butyric acid methyl ester solution on the interface passivation layer, with the parameters set to 1500r / m for 30s, and then using an evaporation coating machine to evaporate a layer of 8nm thick bathocuproin on it to obtain an electron transport layer;
[0027] 9) An evaporation coating machine is used to evaporate a layer of 80 nm thick silver electrode on the surface of the electron transport layer, and finally a perovskite solar cell based on copper-doped lanthanum hydroxide nanomaterials is obtained.
[0028] Beneficial effects:
[0029] 1. The present invention is the first to apply inorganic metal hydroxide nanomaterials as hole transport materials in perovskite solar cells.
[0030] 2. The preparation process of the copper-doped lanthanum hydroxide nanomaterial in the present invention is simple and has good repeatability.
[0031] 3. Compared with other commonly used organic hole transport materials, the copper-doped lanthanum hydroxide nanomaterial in the present invention has low preparation cost and wide sources.
[0032] 4. The perovskite solar cell based on copper-doped lanthanum hydroxide nanomaterial as a hole transport layer in the present invention has excellent performance, good stability and repeatability. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The present invention provides a flowchart of the preparation process of the copper-doped lanthanum hydroxide nanomaterial.
[0034] Figure 2 This is a flowchart of the process for preparing a perovskite solar cell based on copper-doped lanthanum hydroxide nanomaterials as a hole transport layer according to the present invention.
[0035] Figure 3 This is a transmission electron micrograph of the copper-doped lanthanum hydroxide nanomaterial prepared in Example 3.
[0036] Figure 4 This is a scanning electron microscope image of the copper-doped lanthanum hydroxide nanomaterial prepared in Example 3.
[0037] Figure 5 This is a scanning electron microscope image of the cross section of the perovskite solar cell prepared in Example 3.
[0038] Figure 6 The current density-voltage curves of the perovskite solar cells prepared in Examples 1 to 4 are shown. DETAILED DESCRIPTION
[0039] All features disclosed in this specification, except mutually exclusive features and / or steps, can be combined in any manner.
[0040] The present invention prepares copper-doped lanthanum hydroxide nanomaterials by a hydrothermal method and applies the nanomaterials to perovskite solar cells. The chemicals used mainly include lanthanum nitrate, copper nitrate, potassium hydroxide, lead iodide, lead bromide, methyl iodide, methylamine bromide, cesium iodide, phenethylamine iodide, [6,6]-phenyl C61 butyric acid methyl ester, bathocuproin, polyether P123, ethanol, ethylene glycol, ammonia water, dimethyl sulfoxide, dimethylformamide, isopropanol, hydroxyethyl acrylate, chlorobenzene, etc.
[0041] The present invention is described in detail below by way of examples, the purpose of which is to provide a better understanding of the content of the present invention. The examples given are not intended to limit the protection scope of the present invention.
[0042] Example 1
[0043] A method for preparing a lanthanum hydroxide nanomaterial and applying the lanthanum hydroxide nanomaterial as a hole transport material in a perovskite solar cell comprises the following steps:
[0044] This embodiment is a control example, and its main features are: the hole transport material used in the perovskite solar cell is a lanthanum hydroxide nanomaterial not doped with copper.
[0045] (1) A method for preparing lanthanum hydroxide nanomaterial
[0046] Dissolve 0.7g potassium hydroxide in 25mL deionized water and ultrasonicate for 15min. Dissolve 1g polyether P123 in 20mL deionized water and stir for 12h. Dissolve 1.28mmol lanthanum nitrate in 4mL of the polyether P123 solution prepared above and stir for 5min. Then add 3.5mL ethylene glycol and 8mL of the potassium hydroxide solution prepared above dropwise to the above solution and continue stirring for more than 40min. After stirring, transfer the above solution to a reactor and perform hydrothermal reaction at 210℃ for 50min. After the hydrothermal reaction is completed and the reactor is cooled, remove the supernatant by centrifugation to obtain a crude product. Then wash the reaction product with dilute ammonia water and isopropanol in turn to finally obtain lanthanum hydroxide nanomaterials.
[0047] (2) Method for applying the above lanthanum hydroxide nanomaterial to perovskite solar cells
[0048] The etched 1.5cm×1.5cm fluorine-doped tin dioxide conductive glass substrate was cleaned with isopropanol, deionized water, and ethanol for 20 minutes, and then dried with a nitrogen gun. Then UV ozone for 15 minutes. The prepared lanthanum hydroxide nanomaterial was dispersed in a mixed solvent of isopropanol and dimethyl sulfoxide with a volume ratio of 1:1 at a concentration of 6.5mg / mL. The solution was then spin-coated on the fluorine-doped tin dioxide conductive glass substrate with a drop amount of 45μL, a spin coating speed of 7000r / min, and a spin coating time of 50s. After the spin coating is completed, it is placed on a heating plate at 100℃ for annealing for 10 minutes. Repeat this process 4 times to finally obtain a hole transport layer. 80 mg of lead bromide, 66 mg of cesium iodide, 568 mg of lead iodide, 12 mg of methyl bromide, and 187 mg of iodoformamide were dissolved in a mixed solvent of 800 μL of dimethyl sulfoxide and 200 μL of dimethylformamide. After uniform dissolution, 10 μL of hydroxyethyl acrylate was added to prepare a perovskite precursor solution. The solution was then added in a drop amount of 45 μL, and the perovskite precursor solution was spin-coated on top of the hole transport layer using a two-step spin coating method. The first step of the spin coating parameters were a spin coating speed of 500 r / min and a spin coating time of 5 s. The second step of the spin coating parameters were a spin coating speed of 5000 r / min and a spin coating time of 45 s. 30 s before the end of the second step of the spin coating, 100 μL of chlorobenzene antisolvent was added. After the spin coating was completed, it was placed on a heating plate at 100 ° C for annealing for 10 minutes to finally obtain a perovskite layer. Dissolve 0.5 mg of phenylethylamine iodide in 500 μL of isopropanol and stir for 30 min. Then spin coat the solution on the perovskite layer with a drop amount of 50 uL, a spin coating speed of 4000 r / min, and a spin coating time of 30 s. After the spin coating is completed, place it on a 100 ° C hot plate for annealing for 10 min to obtain an interface passivation layer. Dissolve 10 mg of [6,6]-phenyl C61 butyric acid methyl ester in 500 μL of chlorobenzene and stir for 6 h. Then spin coat the solution on the interface passivation layer with a drop amount of 40 uL, a spin coating speed of 1500 r / min, and a spin coating time of 30 s. Then use an evaporation coating machine to evaporate 8 nm thick bathocuproin to obtain an electron transport layer. Finally, use an evaporation coating machine to evaporate 80 nm thick silver electrode to obtain a silver electrode layer. Finally, a perovskite solar cell based on lanthanum hydroxide nanomaterials as a hole transport layer is obtained. The current density-voltage curve of the device was tested (the test condition was a light intensity of 100 mW cm -2 AM 1.5 simulated sunlight), the curve is as follows Figure 6 The test results are shown in Table 1.
[0049] Example 2
[0050] A method for preparing a copper-doped lanthanum hydroxide nanomaterial and applying the same as a hole transport material to a perovskite solar cell comprises the following steps:
[0051] The main feature of this embodiment is that when hydrothermally synthesizing copper-doped lanthanum hydroxide nanomaterials, the feed amount of copper nitrate is 10% of lanthanum nitrate.
[0052] (1) A method for preparing copper-doped lanthanum hydroxide nanomaterial
[0053] Dissolve 0.7g potassium hydroxide in 25mL deionized water and ultrasonicate for 15min. Dissolve 1g polyether P123 in 20mL deionized water and stir for 12h. Dissolve 1.28mmol lanthanum nitrate and 0.128mmol copper nitrate in 4mL of the polyether P123 solution prepared above and stir for 5min. Then add 3.5mL ethylene glycol and 8mL of the potassium hydroxide solution prepared above dropwise to the above solution and continue stirring for more than 40min. After stirring, transfer the above solution to a reactor and perform hydrothermal reaction at 210℃ for 50min. After the hydrothermal reaction is completed and the reactor is cooled, remove the supernatant by centrifugation to obtain a crude product. Then wash the reaction product with dilute ammonia water and isopropanol in turn to obtain copper-doped lanthanum hydroxide nanomaterials.
[0054] (2) Method for applying the above copper-doped lanthanum hydroxide nanomaterial to perovskite solar cells
[0055] The etched 1.5cm×1.5cm fluorine-doped tin dioxide conductive glass substrate was cleaned with isopropanol, deionized water, and ethanol for 20 minutes, and then dried with a nitrogen gun. Then UV ozone treatment for 15 minutes. The copper-doped lanthanum hydroxide nanomaterial prepared above was dispersed in a mixed solvent of isopropanol and dimethyl sulfoxide with a volume ratio of 1:1 at a concentration of 6.5mg / mL. The solution was then spin-coated on the fluorine-doped tin dioxide conductive glass substrate with a drop amount of 45μL, a spin coating speed of 7000r / min, and a spin coating time of 50s. After the spin coating is completed, it is placed on a heating plate at 100℃ for annealing for 10 minutes. Repeat this process 4 times to finally obtain a hole transport layer. 80 mg of lead bromide, 66 mg of cesium iodide, 568 mg of lead iodide, 12 mg of methyl bromide, and 187 mg of iodoformamide were dissolved in a mixed solvent of 800 μL of dimethyl sulfoxide and 200 μL of dimethylformamide. After uniform dissolution, 10 μL of hydroxyethyl acrylate was added to prepare a perovskite precursor solution. The solution was then added in a drop amount of 45 μL, and the perovskite precursor solution was spin-coated on top of the hole transport layer using a two-step spin coating method. The first step of the spin coating parameters were a spin coating speed of 500 r / min and a spin coating time of 5 s. The second step of the spin coating parameters were a spin coating speed of 5000 r / min and a spin coating time of 45 s. 30 s before the end of the second step of the spin coating, 100 μL of chlorobenzene antisolvent was added. After the spin coating was completed, it was placed on a heating plate at 100 ° C for annealing for 10 minutes to finally obtain a perovskite layer. Dissolve 0.5 mg of phenylethylamine iodide in 500 μL of isopropanol and stir for 30 min. Then spin coat the solution on the perovskite layer with a drop amount of 50 uL, a spin coating speed of 4000 r / min, and a spin coating time of 30 s. After the spin coating is completed, place it on a 100 ° C hot plate for annealing for 10 min to obtain an interface passivation layer. Dissolve 10 mg of [6,6]-phenyl C61 butyric acid methyl ester in 500 μL of chlorobenzene and stir for 6 h. Then spin coat the solution on the interface passivation layer with a drop amount of 40 uL, a spin coating speed of 1500 r / min, and a spin coating time of 30 s. Then use an evaporation coating machine to evaporate 8 nm thick bath copper to obtain an electron transport layer. Finally, use an evaporation coating machine to evaporate 80 nm thick silver electrode to obtain a silver electrode layer. Finally, a perovskite solar cell based on copper-doped lanthanum hydroxide nanomaterials as a hole transport layer is obtained. The current density-voltage curve of the device was tested (the test condition was a light intensity of 100 mW cm -2 AM 1.5 simulated sunlight), the curve is as follows Figure 6 The test results are shown in Table 1.
[0056] Example 3
[0057] A method for preparing a copper-doped lanthanum hydroxide nanomaterial and applying the same as a hole transport material to a perovskite solar cell comprises the following steps:
[0058] The main feature of this embodiment is that when hydrothermally synthesizing copper-doped lanthanum hydroxide nanomaterials, the amount of copper nitrate added is 25% of lanthanum nitrate. This embodiment is the embodiment with the highest performance in preparing perovskite solar cells.
[0059] (1) A method for preparing copper-doped lanthanum hydroxide nanomaterial
[0060] Dissolve 0.7g potassium hydroxide in 25mL deionized water and ultrasonicate for 15min. Dissolve 1g polyether P123 in 20mL deionized water and stir for 12h. Dissolve 1.28mmol lanthanum nitrate and 0.32mmol copper nitrate in 4mL of the polyether P123 solution prepared above and stir for 5min. Then add 3.5mL ethylene glycol and 8mL of the potassium hydroxide solution prepared above dropwise to the above solution and continue stirring for more than 40min. After stirring, transfer the above solution to a reactor and perform hydrothermal reaction at 210℃ for 50min. After the hydrothermal reaction is completed and the reactor is cooled, remove the supernatant by centrifugation to obtain a crude product. Then wash the reaction product with dilute ammonia water and isopropanol in turn to finally obtain copper-doped lanthanum hydroxide nanomaterials. Its transmission electron microscope image is as follows Figure 3 The scanning electron microscope image is shown in Figure 4 shown.
[0061] (2) Method for applying the above copper-doped lanthanum hydroxide nanomaterial to perovskite solar cells
[0062] The etched 1.5cm×1.5cm fluorine-doped tin dioxide conductive glass substrate was cleaned with isopropanol, deionized water, and ethanol for 20 minutes, and then dried with a nitrogen gun. Then UV ozone for 15 minutes. The copper-doped lanthanum hydroxide nanomaterial prepared above was dispersed in a mixed solvent of isopropanol and dimethyl sulfoxide with a volume ratio of 1:1 at a concentration of 6.5mg / mL. The solution was then spin-coated on the fluorine-doped tin dioxide conductive glass substrate with a drop amount of 45μL, a spin coating speed of 7000r / min, and a spin coating time of 50s. After the spin coating is completed, it is placed on a heating plate at 100℃ for annealing for 10 minutes. Repeat this process 4 times to finally obtain a hole transport layer. 80 mg of lead bromide, 66 mg of cesium iodide, 568 mg of lead iodide, 12 mg of methyl bromide, and 187 mg of iodoformamide were dissolved in a mixed solvent of 800 μL of dimethyl sulfoxide and 200 μL of dimethylformamide. After uniform dissolution, 10 μL of hydroxyethyl acrylate was added to prepare a perovskite precursor solution. The solution was then added in a drop amount of 45 μL, and the perovskite precursor solution was spin-coated on top of the hole transport layer using a two-step spin coating method. The first step of the spin coating parameters were a spin coating speed of 500 r / min and a spin coating time of 5 s. The second step of the spin coating parameters were a spin coating speed of 5000 r / min and a spin coating time of 45 s. 30 s before the end of the second step of the spin coating, 100 μL of chlorobenzene antisolvent was added. After the spin coating was completed, it was placed on a heating plate at 100 ° C for annealing for 10 minutes to finally obtain a perovskite layer. Dissolve 0.5 mg of phenylethylamine iodide in 500 μL of isopropanol and stir for 30 minutes. Then spin-coat the solution on top of the perovskite layer with a drop amount of 50 uL, a spin coating speed of 4000 r / min, and a spin coating time of 30 seconds. After the spin coating is completed, anneal it on a 100°C hot plate for 10 minutes to obtain an interface passivation layer. Dissolve 10 mg of [6,6]-phenyl C61 butyric acid methyl ester in 500 μL of chlorobenzene and stir for 6 hours. Then spin-coat the solution on top of the interface passivation layer with a drop amount of 40 uL, a spin coating speed of 1500 r / min, and a spin coating time of 30 seconds. Then use an evaporation coating machine to evaporate 8 nm thick bath copper to obtain an electron transport layer. Finally, use an evaporation coating machine to evaporate 80 nm thick silver electrodes to obtain a silver electrode layer. Finally, a perovskite solar cell based on copper-doped lanthanum hydroxide nanomaterials as a hole transport layer is obtained. The scanning electron microscope image of the cross section of the device is as follows Figure 5 The current density-voltage curve of the device was tested (the test condition was a light intensity of 100 mW cm -2 AM 1.5 simulated sunlight), the curve is as follows Figure 6 The test results are shown in Table 1.
[0063] Example 4
[0064] A method for preparing a copper-doped lanthanum hydroxide nanomaterial and applying the same as a hole transport material to a perovskite solar cell comprises the following steps:
[0065] The main feature of this embodiment is that when hydrothermally synthesizing copper-doped lanthanum hydroxide nanomaterials, the feed amount of copper nitrate is 40% of lanthanum nitrate.
[0066] (1) A method for preparing copper-doped lanthanum hydroxide nanomaterial
[0067] Dissolve 0.7g potassium hydroxide in 25mL deionized water and ultrasonicate for 15min. Dissolve 1g polyether P123 in 20mL deionized water and stir for 12h. Dissolve 1.28mmol lanthanum nitrate and 0.512mmol copper nitrate in 4mL of the polyether P123 solution prepared above and stir for 5min. Then add 3.5mL ethylene glycol and 8mL of the potassium hydroxide solution prepared above dropwise to the above solution and continue stirring for more than 40min. After stirring, transfer the above solution to a reactor and perform hydrothermal reaction at 210℃ for 50min. After the hydrothermal reaction is completed and the reactor is cooled, remove the supernatant by centrifugation to obtain a crude product. Then wash the reaction product with dilute ammonia water and isopropanol in turn to obtain copper-doped lanthanum hydroxide nanomaterials.
[0068] (2) Method for applying the above copper-doped lanthanum hydroxide nanomaterial to perovskite solar cells
[0069] The etched 1.5cm×1.5cm fluorine-doped tin dioxide conductive glass substrate was cleaned with isopropanol, deionized water, and ethanol for 20 minutes, and then dried with a nitrogen gun. Then UV ozone for 15 minutes. The copper-doped lanthanum hydroxide nanomaterial prepared above was dispersed in a mixed solvent of isopropanol and dimethyl sulfoxide with a volume ratio of 1:1 at a concentration of 6.5mg / mL. The solution was then spin-coated on the fluorine-doped tin dioxide conductive glass substrate with a drop amount of 45μL, a spin coating speed of 7000r / min, and a spin coating time of 50s. After the spin coating is completed, it is placed on a heating plate at 100℃ for annealing for 10 minutes. Repeat this process 4 times to finally obtain a hole transport layer. 80 mg of lead bromide, 66 mg of cesium iodide, 568 mg of lead iodide, 12 mg of methyl bromide, and 187 mg of iodoformamide were dissolved in a mixed solvent of 800 μL of dimethyl sulfoxide and 200 μL of dimethylformamide. After uniform dissolution, 10 μL of hydroxyethyl acrylate was added to prepare a perovskite precursor solution. The solution was then added in a drop amount of 45 μL, and the perovskite precursor solution was spin-coated on top of the hole transport layer using a two-step spin coating method. The first step of the spin coating parameters were a spin coating speed of 500 r / min and a spin coating time of 5 s. The second step of the spin coating parameters were a spin coating speed of 5000 r / min and a spin coating time of 45 s. 30 s before the end of the second step of the spin coating, 100 μL of chlorobenzene antisolvent was added. After the spin coating was completed, it was placed on a heating plate at 100 ° C for annealing for 10 minutes to finally obtain a perovskite layer. Dissolve 0.5 mg of phenylethylamine iodide in 500 μL of isopropanol and stir for 30 min. Then spin coat the solution on the perovskite layer with a drop amount of 50 uL, a spin coating speed of 4000 r / min, and a spin coating time of 30 s. After the spin coating is completed, place it on a 100 ° C hot plate for annealing for 10 min to obtain an interface passivation layer. Dissolve 10 mg of [6,6]-phenyl C61 butyric acid methyl ester in 500 μL of chlorobenzene and stir for 6 h. Then spin coat the solution on the interface passivation layer with a drop amount of 40 uL, a spin coating speed of 1500 r / min, and a spin coating time of 30 s. Then use an evaporation coating machine to evaporate 8 nm thick bath copper to obtain an electron transport layer. Finally, use an evaporation coating machine to evaporate 80 nm thick silver electrode to obtain a silver electrode layer. Finally, a perovskite solar cell based on copper-doped lanthanum hydroxide nanomaterials as a hole transport layer is obtained. The current density-voltage curve of the device was tested (the test condition was a light intensity of 100 mW cm -2 AM 1.5 simulated sunlight), the curve is as follows Figure 6 The test results are shown in Table 1.
[0070] Example 5
[0071] A method for preparing a copper-doped lanthanum hydroxide nanomaterial and applying the same as a hole transport material to a perovskite solar cell comprises the following steps:
[0072] The main feature of this embodiment is that when preparing the hole transport layer of the perovskite solar cell, the process of spin coating and annealing the hole transport material is repeated 3 times.
[0073] (1) A method for preparing copper-doped lanthanum hydroxide nanomaterial
[0074] Dissolve 0.7g potassium hydroxide in 25mL deionized water and ultrasonicate for 15min. Dissolve 1g polyether P123 in 20mL deionized water and stir for 12h. Dissolve 1.28mmol lanthanum nitrate and 0.32mmol copper nitrate in 4mL of the polyether P123 solution prepared above and stir for 5min. Then add 3.5mL ethylene glycol and 8mL of the potassium hydroxide solution prepared above dropwise to the above solution and continue stirring for more than 40min. After stirring, transfer the above solution to a reactor and perform hydrothermal reaction at 210℃ for 50min. After the hydrothermal reaction is completed and the reactor is cooled, remove the supernatant by centrifugation to obtain a crude product. Then wash the reaction product with dilute ammonia water and isopropanol in turn to obtain copper-doped lanthanum hydroxide nanomaterials.
[0075] (2) Method for applying the above copper-doped lanthanum hydroxide nanomaterial to perovskite solar cells
[0076] The etched 1.5cm×1.5cm fluorine-doped tin dioxide conductive glass substrate was cleaned with isopropanol, deionized water, and ethanol for 20 minutes, and then dried with a nitrogen gun. Then UV ozone for 15 minutes. The copper-doped lanthanum hydroxide nanomaterial prepared above was dispersed in a mixed solvent of isopropanol and dimethyl sulfoxide with a volume ratio of 1:1 at a concentration of 6.5mg / mL. The solution was then spin-coated on the fluorine-doped tin dioxide conductive glass substrate with a drop amount of 45μL, a spin coating speed of 7000r / min, and a spin coating time of 50s. After the spin coating is completed, it is placed on a heating plate at 100℃ for annealing for 10 minutes. Repeat this process 3 times to finally obtain a hole transport layer.
[0077] 80 mg of lead bromide, 66 mg of cesium iodide, 568 mg of lead iodide, 12 mg of methyl bromide, and 187 mg of iodoformamide were dissolved in a mixed solvent of 800 μL of dimethyl sulfoxide and 200 μL of dimethylformamide. After uniform dissolution, 10 μL of hydroxyethyl acrylate was added to prepare a perovskite precursor solution. The solution was then added in a drop amount of 45 μL, and the perovskite precursor solution was spin-coated on top of the hole transport layer using a two-step spin coating method. The first step of the spin coating parameters were a spin coating speed of 500 r / min and a spin coating time of 5 s. The second step of the spin coating parameters were a spin coating speed of 5000 r / min and a spin coating time of 45 s. 30 s before the end of the second step of the spin coating, 100 μL of chlorobenzene antisolvent was added. After the spin coating was completed, it was placed on a heating plate at 100 ° C for annealing for 10 minutes to finally obtain a perovskite layer.
[0078] Dissolve 0.5 mg of phenethylamine iodide in 500 μL of isopropanol and stir for 30 minutes. Then spin-coat the solution on the perovskite layer with a drop amount of 50 μL, a spin-coating speed of 4000 r / min, and a spin-coating time of 30 seconds. After the spin-coating is completed, anneal on a 100°C hot plate for 10 minutes to obtain an interface passivation layer.
[0079] Dissolve 10 mg of [6,6]-phenyl C61 butyric acid methyl ester in 500 μL of chlorobenzene and stir for 6 hours. Then spin coat the solution on the interface passivation layer with a drop amount of 40 μL, a spin coating speed of 1500 r / min, and a spin coating time of 30 seconds. Then use an evaporation coating machine to evaporate 8 nm thick bathocuproin to obtain an electron transport layer.
[0080] Finally, an 80nm thick silver electrode was deposited using an evaporation coating machine to obtain a silver electrode layer. Finally, a perovskite solar cell based on copper-doped lanthanum hydroxide nanomaterials as a hole transport layer was obtained. The current density-voltage curve of the device (test condition: light intensity of 100mWcm -2 The test results of the AM 1.5 simulated sunlight irradiation are shown in Table 2.
[0081] Example 6
[0082] A method for preparing a copper-doped lanthanum hydroxide nanomaterial and applying the same as a hole transport material to a perovskite solar cell comprises the following steps:
[0083] The main feature of this embodiment is that when preparing the hole transport layer of the perovskite solar cell, the process of spin coating and annealing the hole transport material is repeated 5 times.
[0084] (1) A method for preparing copper-doped lanthanum hydroxide nanomaterial
[0085] Dissolve 0.7g potassium hydroxide in 25mL deionized water and ultrasonicate for 15min. Dissolve 1g polyether P123 in 20mL deionized water and stir for 12h. Dissolve 1.28mmol lanthanum nitrate and 0.32mmol copper nitrate in 4mL of the polyether P123 solution prepared above and stir for 5min. Then add 3.5mL ethylene glycol and 8mL of the potassium hydroxide solution prepared above dropwise to the above solution and continue stirring for more than 40min. After stirring, transfer the above solution to a reactor and perform hydrothermal reaction at 210℃ for 50min. After the hydrothermal reaction is completed and the reactor is cooled, remove the supernatant by centrifugation to obtain a crude product. Then wash the reaction product with dilute ammonia water and isopropanol in turn to obtain copper-doped lanthanum hydroxide nanomaterials.
[0086] (2) Method for applying the above copper-doped lanthanum hydroxide nanomaterial to perovskite solar cells
[0087] The etched 1.5cm×1.5cm fluorine-doped tin dioxide conductive glass substrate was cleaned with isopropanol, deionized water, and ethanol for 20 minutes, and then dried with a nitrogen gun. Then UV ozone for 15 minutes. The copper-doped lanthanum hydroxide nanomaterial prepared above was dispersed in a mixed solvent of isopropanol and dimethyl sulfoxide with a volume ratio of 1:1 at a concentration of 6.5mg / mL. The solution was then spin-coated on the fluorine-doped tin dioxide conductive glass substrate with a drop amount of 45μL, a spin coating speed of 7000r / min, and a spin coating time of 50s. After the spin coating is completed, it is placed on a heating plate at 100℃ for annealing for 10 minutes. Repeat this process 5 times to finally obtain a hole transport layer. 80 mg of lead bromide, 66 mg of cesium iodide, 568 mg of lead iodide, 12 mg of methyl bromide, and 187 mg of iodoformamide were dissolved in a mixed solvent of 800 μL of dimethyl sulfoxide and 200 μL of dimethylformamide. After uniform dissolution, 10 μL of hydroxyethyl acrylate was added to prepare a perovskite precursor solution. The solution was then added in a drop amount of 45 μL, and the perovskite precursor solution was spin-coated on top of the hole transport layer using a two-step spin coating method. The first step of the spin coating parameters were a spin coating speed of 500 r / min and a spin coating time of 5 s. The second step of the spin coating parameters were a spin coating speed of 5000 r / min and a spin coating time of 45 s. 30 s before the end of the second step of the spin coating, 100 μL of chlorobenzene antisolvent was added. After the spin coating was completed, it was placed on a heating plate at 100 ° C for annealing for 10 minutes to finally obtain a perovskite layer. Dissolve 0.5 mg of phenylethylamine iodide in 500 μL of isopropanol and stir for 30 min. Then spin coat the solution on the perovskite layer with a drop amount of 50 uL, a spin coating speed of 4000 r / min, and a spin coating time of 30 s. After the spin coating is completed, place it on a 100 ° C hot plate for annealing for 10 min to obtain an interface passivation layer. Dissolve 10 mg of [6,6]-phenyl C61 butyric acid methyl ester in 500 μL of chlorobenzene and stir for 6 h. Then spin coat the solution on the interface passivation layer with a drop amount of 40 uL, a spin coating speed of 1500 r / min, and a spin coating time of 30 s. Then use an evaporation coating machine to evaporate 8 nm thick bath copper to obtain an electron transport layer. Finally, use an evaporation coating machine to evaporate 80 nm thick silver electrode to obtain a silver electrode layer. Finally, a perovskite solar cell based on copper-doped lanthanum hydroxide nanomaterials as a hole transport layer is obtained. The current density-voltage curve of the device (test condition: light intensity is 100mWcm -2 The test results of the AM 1.5 simulated sunlight irradiation are shown in Table 2.
[0088] Table 1 Performance of perovskite solar cells with hole transport layers prepared based on different copper nitrate feed ratios
[0089]
[0090] Table 2 Performance of perovskite solar cells based on hole transport layers with different spin coating times
[0091]
[0092] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto, and any changes or substitutions that are not conceived by creative work should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope defined in the claims.
Claims
1. A method for preparing a copper-doped lanthanum hydroxide nanomaterial, comprising the following steps: 1) Prepare a 50 mg / mL polyether P123 solution with deionized water; 2) Mix the lanthanum source material and the copper source material into a beaker, wherein the molar amount of copper in the material is 10-40% of the lanthanum, add the polyether P123 solution prepared in step 1), and stir to form a uniform mixed solution; wherein, for every 1 mmol La 3+ Use 3.125 mL of polyether P123 solution; 3) Slowly add ethylene glycol to the solution obtained in step 2) and continue stirring to form a uniform mixed solution; wherein, for every 1 mmol La 3+ Use 2.734 mL of ethylene glycol; 4) Prepare a 0.5M potassium hydroxide solution with deionized water; 5) Under stirring conditions, slowly add the prepared potassium hydroxide solution to the solution obtained in step 3) and stir to form a uniform mixed solution; wherein, for every 1 mmol La 3+ Use 6.25mL of potassium hydroxide solution; 6) Transfer the solution obtained in step 5) to a reactor and heat at 210 degrees Celsius for 50 minutes; 7) After the hydrothermal reaction in step 6) is completed and the reactor is cooled, the supernatant is removed by centrifugation to obtain a crude product, and the reaction product is then washed with dilute ammonia water and isopropanol in sequence to finally obtain copper-doped lanthanum hydroxide nanomaterials.
2. The method for preparing a copper-doped lanthanum hydroxide nanomaterial according to claim 1, characterized in that: The lanthanum source material and the copper source material in step 2) are lanthanum nitrate and copper nitrate, and the molar amount of copper nitrate is 25% of that of lanthanum nitrate.
3. An application of the copper-doped lanthanum hydroxide nanomaterial prepared by the preparation method according to claim 1, which is to apply the copper-doped lanthanum hydroxide nanomaterial prepared by the preparation method according to claim 1 as a hole transport layer to a perovskite solar cell, wherein the preparation method of the perovskite solar cell comprises the following steps: 1) The etched 1.5 cm × 1.5 cm fluorine-doped tin dioxide conductive glass substrate was ultrasonically cleaned in isopropanol, deionized water, and ethanol for 15 min, and then treated with UV ozone for 15 min; 2) The copper-doped lanthanum hydroxide nanomaterial is dispersed in a mixed solvent of dimethyl sulfoxide and isopropanol in a volume ratio of 1:1 using a cell crusher, and then spin-coated on a transparent conductive glass substrate. The spin-coating parameters are set as follows: a spin-coating speed of 7000 rpm and a spin-coating time of 50 s. After the spin-coating is completed, it is placed on a heating plate at 100° C. for annealing for 10 minutes. The spin-coating and annealing process is repeated four times to obtain a hole transport layer; 3) Mix methylamine bromide, lead bromide, cesium iodide, iodoformamide, and lead iodide in a molar ratio of 1:1.9:2.3:10:11.4, and then dissolve in a mixed solvent of dimethylformamide and dimethyl sulfoxide in a volume ratio of 4:1, using 9.2 mL of the mixed solvent for every 1 mmol of methylamine bromide, and finally add 1% of the total volume of the mixed solvent. Hydroxyethyl acrylate is added and mixed evenly to obtain a perovskite precursor solution; 4) Spin coating the perovskite precursor solution on the hole transport layer by a two-step spin coating method, with the parameters set as follows: the first step is a spin coating speed of 500 rpm and a spin coating time of 5 s, and the second step is a spin coating speed of 5000 rpm and a spin coating time of 45 s; 30 s before the end of spin coating, 100 uL of chlorobenzene antisolvent is added dropwise, and after the spin coating is completed, annealing is performed on a 100° C. hot plate for 10 min to obtain a perovskite layer; 5) Prepare a 1 mg / mL solution of phenethylammonium iodide in isopropanol. 6) Spin-coat the phenylethyl ammonium iodide solution on the perovskite layer, and set the parameters as follows: 4000 rpm spin-coating speed, 30 s spin-coating time, and anneal on a 100°C hot plate for 10 min after spin-coating to obtain an interface passivation layer; 7) Prepare a 20 mg / mL solution of [6,6]-phenyl C61 butyric acid methyl ester using chlorobenzene as solvent; 8) Spin-coat the [6,6]-phenyl C61 butyric acid methyl ester solution on the interface passivation layer, with the parameters set as: 1500 rpm spin coating speed, 30 s spin coating time, and then use an evaporation coating machine to evaporate a layer of 8 nm thick bathocuproin on it to obtain an electron transport layer; 9) An evaporation coating machine was used to evaporate a layer of 80 nm thick silver electrode on the surface of the electron transport layer to obtain a perovskite solar cell based on copper-doped lanthanum hydroxide nanomaterials.
Citation Information
Patent Citations
Rare earth element-doped layered composite metal hydroxide and preparation and application thereof
CN109289857A
Gamma-Ga2O3 or Cu-doped gamma-Ga2O3 nanocrystal as well as preparation method and application thereof
CN114086238A