Repairable graphite mold blank, forming mold, repairing agent and repairing method

Through the combination of graphite mold blank and repair agent, the problems of inaccurate size, difficult to repair and high cost in the hot press tank molding process are solved, and high strength, high hardness, and reusable mold preparation is achieved. Suitable for complex shapes and hot press tank forming processes.

CN116496084BActive Publication Date: 2024-11-22上海晋飞碳纤科技股份有限公司
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202310241488.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-14
Publication Date
2024-11-22
Estimated Expiration
2043-03-14

AI Technical Summary

Technical Problem

In the hot press tank molding process, existing mold materials have problems such as inaccurate size, difficult to repair, high cost and large weight, especially in the process of complex shape molds, and the accuracy is reduced after repair.

Method used

Repairable mold blanks mainly composed of graphite are prepared by thermal isostatic molding through raw materials such as dry asphalt, graphite, elemental silicon and phenolic resin to prepare high-strength and high-hardness mold blanks, and are equipped with graphite material repair agents. Repair to realize the reuse of the mold.

Benefits of technology

It obtains a mold with light weight, reusability, high precision and convenient repair. It is suitable for complex shapes and hot press tank molding processes, reducing production costs and difficulty in obtaining materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004292018590000071
    Figure GDA0004292018590000071
  • Figure GDA0004292018590000081
    Figure GDA0004292018590000081
Patent Text Reader

Abstract

The invention provides a repairable graphite mold blank, a molding mold, a repairing agent and a repairing method. The repairable graphite mold blank uses a mixture of 1-10% dry asphalt, 60-90% graphite, 1-10% mold waste, 1-5% elemental silicon and 1-10% phenolic resin as raw materials, and the graphite mold blank is obtained by controlling the sintering temperature of the hot isostatic pressing process to 1600-2400°C and the sintering time to 0.5-2 hours. The graphite mold blank can be used to prepare a molding mold with a complex shape, and the mold has the advantages of being light, reusable and easy to repair.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite material molds, and in particular to a repairable graphite mold blank, a forming mold, a repairing agent and a repairing method. Background Art

[0002] Mold forming is the main means of forming carbon fiber resin composite materials. In the autoclave forming process, the composite blank formed by stacking a single layer of prepreg in a predetermined direction is placed in the autoclave to complete the curing process at a certain temperature and pressure. The autoclave is a special pressure vessel that can withstand and regulate a certain temperature and pressure range. The blank is laid on the surface of the mold with a release agent, and then covered with porous anti-stick cloth (film), adhesive felt, and breathable felt in turn, and sealed in a vacuum bag, and then placed in the autoclave. Before heating and curing, the bag is first evacuated to remove air and volatiles, and then heated, pressurized, and cured according to the curing system of different resins. The formulation and implementation of the curing process are the key to ensuring the quality of autoclave molded parts. This molding process is suitable for the manufacture of aircraft doors, fairings, airborne radar covers, including frames, wings, tail fins and other products.

[0003] Having a suitable mold is an important step in composite material molding. When designing a mold, the following requirements must be considered comprehensively: ① Meet the precision requirements of product design, the mold size is accurate and the surface is smooth; ② Sufficient strength and rigidity; ③ Convenient demoulding; ④ Sufficient thermal stability; ⑤ Light weight, sufficient material source and low cost. When choosing the material for making the mold, the following factors should be considered: ① The mold material must have sufficient strength and rigidity to ensure that the mold is not easily deformed or damaged during use; ② Good heat resistance, the mold is not easily deformed when the product is cured and heated; ③ Easy to manufacture and easy to demould; ④ Try to reduce the weight of the mold to facilitate production; ⑤ Low price and easy to obtain materials.

[0004] Materials suitable for autoclave molding molds include: bakelite, glass, gypsum, metal, fiberglass, carbon fiber, etc. However, there are certain limitations in using the above materials to make molds. For example, bakelite surface requirements are not easy to meet, gypsum is easily damaged and cannot be reused, metal has too large a specific gravity, fiberglass has too large thermal expansion, carbon fiber is too expensive, glass is not easy to prepare complex shapes, etc. In addition, molds made of the above materials are difficult to repair when damaged, and the precision of the repaired molds is reduced. Therefore, there is an urgent need for a mold that can be applied to the autoclave molding process. Summary of the invention

[0005] In view of this, the embodiments of the present specification provide a repairable graphite mold blank, a molding mold, a repair agent and a repair method, wherein the repairable graphite mold blank can be prepared into complex shapes and adapt to the autoclave molding process. The molding mold made using the blank has the advantages of being light, reusable and easy to repair.

[0006] The embodiments of this specification provide the following technical solutions:

[0007] A repairable graphite mold blank, the raw materials for preparing the graphite mold blank include:

[0008] In terms of mass percentage, dry asphalt 1-10%, graphite 60-90%, mold waste 1-10%, elemental silicon 1-5%, phenolic resin 1-10%;

[0009] The preparation method thereof comprises the following steps:

[0010] The raw materials are mixed uniformly and then hot isostatically pressed to obtain the graphite mold blank, wherein the sintering temperature is 1600-2400° C. and the sintering time is 0.5-2 hours.

[0011] The above-mentioned graphite mold blank is directly powder-formed by hot isostatic pressing. The formula raw materials are easy to obtain and low in cost, and are suitable for industrial use. The formula raw materials are subjected to high temperature and high pressure, and the products are sintered and densified to obtain high-performance new material blanks with high strength and high hardness, which are convenient for subsequent processing into molding molds. The molds produced have the advantages of light weight, reusability and easy repair.

[0012] The embodiment of this specification also provides a solution, wherein the sintering temperature is 2000-2100° C., and the sintering time is 0.8-1.2 hours.

[0013] The embodiments of the present specification also provide a repairable molding die obtained from any of the aforementioned graphite mold blanks, wherein the graphite mold blank is mechanically processed to obtain a mold assembly, and the mold assembly is at least one and is used to construct the molding die.

[0014] The embodiments of this specification also provide a solution, wherein the machining includes turning or wire cutting.

[0015] The embodiment of this specification also provides a solution, the accuracy of the repairable molding die is between 0.03-0.15mm, preferably, the accuracy is between 0.04-0.06mm;

[0016] And / or, the density of the repairable molding die is 1-3 g / cm 3 Preferably, the density is between 1.7-1.95 g / cm 3 between;

[0017] And / or, the compressive strength of the repairable forming mold is between 80-90 MPa, preferably, the compressive strength is between 84-87 MPa, measured according to the national standard GB / T7314;

[0018] and / or, the hardness of the repairable forming die is between 34 and 45, preferably, the hardness is between 40 and 42, measured by the Rockwell hardness method;

[0019] And / or, the expansion coefficient of the repairable molding die is between 7 and 15×10 -6 / ℃, preferably, the expansion coefficient is between 8.5 and 12.5×10 -6 / ℃, and can be adjusted according to the composition.

[0020] The embodiment of this specification also provides a graphite material repair agent for repairing any of the aforementioned repairable molding dies, the graphite material repair agent comprising:

[0021] In terms of mass percentage, the silicon dioxide comprises 30-70%, silica sand comprises 10-30%, silica gel comprises 5-20%, polyvinyl alcohol comprises 5-15%, and graphite has a mass equal to the total mass of the materials.

[0022] The embodiments of this specification also provide a solution, wherein the mass percentages of the silicon dioxide, silica sand, silica gel, and polyvinyl alcohol components are between 50-70%, 15-25%, 5-15%, and 5-15%.

[0023] The embodiment of this specification also provides a solution, the graphite material repair agent also includes hydrated sodium silicate, and the weight ratio of the hydrated sodium silicate to the silicon dioxide is between 1:1 and 1:2.

[0024] The embodiment of this specification also provides a solution, the preparation method of the graphite material repair agent comprises the following steps:

[0025] mixing silicon dioxide, silica sand, silica gel and polyvinyl alcohol to obtain a suspension;

[0026] The suspension is mixed with an equal mass of graphite to obtain the graphite material repair agent.

[0027] The present specification also provides a method for repairing a forming mold, comprising the following steps:

[0028] Providing a repairable forming mold as described above;

[0029] Providing a graphite material repairing agent as described above;

[0030] The repairable forming mold is repaired by using the graphite material repair agent and dried at 25-400° C., thereby achieving the reuse of the forming mold.

[0031] Compared with the prior art, the beneficial effects that can be achieved by at least one of the above technical solutions adopted in the embodiments of this specification include at least: the above-mentioned repairable graphite mold blank is directly powder-molded by hot isostatic pressing, and its formula raw materials are easy to obtain and low in cost. By controlling the hot isostatic pressing process parameters, the product is densified to obtain a high-strength, high-hardness, high-performance new material blank. For example, providing pressure to improve the surface quality of the blank, providing a suitable sintering temperature to balance the brittleness and toughness of the blank, and providing a suitable sintering time to ensure the uniformity of the inside of the blank. The blank is easy to process into a forming mold in the subsequent process, and the obtained mold has the advantages of light weight, reusability, and easy repair. DETAILED DESCRIPTION

[0032] Various aspects of the present invention are described in further detail below.

[0033] Unless otherwise defined or indicated, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein can be applied to the method of the present invention.

[0034] Unless otherwise clearly specified and limited, the "or" mentioned in the present invention includes the relationship of "and". The "and" is equivalent to the Boolean logic operator "AND", the "or" is equivalent to the Boolean logic operator "OR", and "AND" is a subset of "OR".

[0035] It is to be understood that although the terms "first", "second", etc. may be used herein to describe different elements, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. Therefore, the first element may be referred to as the second element without departing from the teachings of the present invention.

[0036] In the present invention, the terms "comprising", "including" or "comprising" indicate that various components can be applied together in the mixture or composition of the present invention. Therefore, the terms "consisting mainly of" and "consisting of" are included in the terms "comprising", "including" or "comprising".

[0037] Unless otherwise clearly specified and limited, the terms "connected", "connected" and "connection" in the present invention should be understood in a broad sense, for example, it can be a fixed connection, or it can be connected through an intermediary medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0038] The present invention provides a repairable graphite mold blank, and the raw materials for preparing the blank include:

[0039] 1-10 parts by weight of dry asphalt;

[0040] 60-90 parts by weight of graphite;

[0041] 1-10 parts by weight of mold waste;

[0042] 1-5 parts by weight of elemental silicon;

[0043] and 1-10 parts by weight of phenolic resin.

[0044] The method for preparing the above blank comprises the following steps:

[0045] The raw materials in the above weight proportions are mixed evenly, put into a hot isostatic pressing dry bag, and hot isostatic pressing is performed, that is, a hot isostatic pressing sintering method is used, pressure is provided to the hot isostatic pressing machine, the sintering temperature is controlled to be 1600-2400°C, and the sintering time is 0.5-2 hours to obtain a graphite mold blank.

[0046] The more pressure is applied during the sintering process, the better the surface quality of the mold produced by the mold blank. The surface quality is proportional to the pressure. The hardness of the mold blank is proportional to the sintering temperature, but too high a temperature will make the blank brittle and reduce toughness, so the sintering temperature needs to be controlled between 1600-2400℃, and the preferred temperature is between 2000-2100℃. If the sintering time is too short, the material of the mold blank will be uneven and the mixing will not be sufficient. At the same time, if the sintering time is too long, energy will be wasted, so the sintering time needs to be controlled between 0.5-2 hours, and the preferred time is between 0.8-1.2 hours.

[0047] It should be noted that the mold waste refers to the mold waste formed after the mold made of the blank made by the same raw materials and hot isostatic pressing sintering method is used. When mixing the raw materials, the same weight of graphite can also be used instead of the mold waste.

[0048] The present invention also provides a repairable forming mold, which is made by mechanical processing using any of the above-mentioned repairable graphite mold blanks. After cooling the blank (graphite ingot), the rough shape of the mold is obtained by wire cutting, and then the mold is obtained by mechanical processing (such as turning). The mold may include one or more mold assemblies, each of which can be obtained by mechanically processing the blank (graphite ingot). When there are multiple mold assemblies, the mold for molding is obtained by assembly.

[0049] In some embodiments, the repairable molding die comprises a high-precision die, and the die precision is between 0.03-0.15 mm; preferably, the die precision is between 0.04-0.06 mm.

[0050] In some embodiments, the density of the repairable mold is 1-3 g / cm3 Preferably, the density is between 1.7-1.95g / cm 3 between.

[0051] In some embodiments, the compressive strength of the repairable forming mold is between 80-90 MPa; preferably, the compressive strength is between 84-87 MPa, wherein the compressive strength is measured according to the national standard GB / T7314.

[0052] In some embodiments, the hardness of the repairable molding die is between 34-45; preferably, the hardness is between 40-42, wherein the hardness is measured by the Rockwell hardness method.

[0053] In some embodiments, the expansion coefficient of the repairable molding die is between 7 and 15×10 -6 / ℃; preferably, the expansion coefficient is between 8.5 and 12.5×10 -6 / ℃, and can be adjusted according to the composition.

[0054] The present invention also provides a graphite material repairing agent for repairing any one of the above-mentioned repairable forming molds, the repairing agent comprising:

[0055] 30-70 parts by weight of silicon dioxide;

[0056] 10-30 parts by weight of silica sand;

[0057] 5-20 parts by weight of silica gel;

[0058] 5-15 parts by weight of polyvinyl alcohol;

[0059] and graphite having a weight equal to the total weight of the materials.

[0060] Preferably, the graphite material repair agent composition includes:

[0061] 50-70 parts by weight of silicon dioxide;

[0062] 15-25 parts by weight of silica sand;

[0063] 5-15 parts by weight of silica gel;

[0064] 5-15 parts by weight of polyvinyl alcohol;

[0065] and graphite having a weight equal to the total weight of the materials.

[0066] Preferably, the preparation method of the graphite material repair agent comprises the following steps:

[0067] mixing silicon dioxide, silica sand, silica gel and polyvinyl alcohol to obtain a suspension;

[0068] The above suspension is mixed with an equal mass of graphite to obtain a graphite material repair agent.

[0069] Optionally, the graphite material repair agent component also includes hydrated sodium silicate, and the weight ratio of the hydrated sodium silicate to the silicon dioxide is between 1:1 and 1:2.

[0070] The present invention also provides a method for repairing a forming mold, which is used to repair any of the above-mentioned repairable forming molds, comprising the following steps:

[0071] Providing any one of the above repairable forming molds;

[0072] Provide any of the above graphite material repair agents;

[0073] The repairable forming mold is repaired by using a graphite material repair agent and dried at 40-400° C., thereby achieving the effect of reusing the forming mold.

[0074] Embodiment 1:

[0075] Weigh dry asphalt according to proportion, crush it, mix it with graphite, mold waste, elemental silicon, and phenolic resin powder 100g, 1600g, 120g, 40g, 140g, put it into a hot isostatic pressing dry bag, sinter it at 2000℃ for 1 hour, cool it to get graphite ingots, and machine it to get molds. Dry asphalt can be a conventional cold patch asphalt mixture, which refers to a mixture formed by mixing unheated mineral material (aggregate), mineral powder and diluted asphalt. The mineral material can be machine-made sand or natural sand. The mineral powder is made by grinding limestone. The mixing ratio of mineral material, mineral powder and asphalt is 80:13:7. Cold patch asphalt mixture can be prepared on site or purchased as a finished product. Graphite is conventional graphite powder, elemental silicon is conventional single crystal silicon powder, and phenolic resin is liquid. Asphalt can also be selected from conventional viscous fluid asphalt, and phenolic resin is selected from powder.

[0076] The repair plan is a liquid mixed solution of 60% silica, 20% silica sand, 10% silica gel, and 10% polyvinyl alcohol. The same weight of graphite powder is added and stirred, and then dried at 140 degrees for 1.5 hours. The hardness is measured to be 45HRB and the surface roughness is Ra1.0.

[0077] Embodiment 2:

[0078] Weigh dry asphalt in proportion, grind it, mix it with graphite, mold waste, elemental silicon, and phenolic resin powder 200g, 3200g, 240g, 80g, and 240g, put it into a hot isostatic pressing dry bag, sinter it at 2100℃ for 1 hour, cool it to get a graphite ingot, and machine it to get a mold.

[0079] The repair plan is a liquid mixed solution of 60% silica, 20% silica sand, 10% silica gel, and 10% polyvinyl alcohol. The same weight of graphite powder is added and stirred, and then dried at 80 degrees for 4.5 hours. The hardness is measured to be 48HRB and the surface roughness is Ra0.4.

[0080] Embodiment 3:

[0081] Weigh dry asphalt in proportion, crush it, mix it with graphite, mold waste, elemental silicon, and phenolic resin powder 200g, 1500g, 120g, 40g, and 140g, put it into a hot isostatic pressing dry bag, sinter it at 2200°C for 0.8 hour, cool it to get a graphite ingot, and machine it to get a mold.

[0082] The repair plan is a liquid mixed solution of 60% silica, 20% silica sand, 10% silica gel, and 10% polyvinyl alcohol. The same weight of graphite powder is added and stirred, and then dried at 25°C for 72 hours. The hardness is measured to be 46.3HRB and the surface roughness is Ra1.2.

[0083] Examples 4 to 8 were prepared according to the following table, and the following hardness and surface roughness were obtained.

[0084]

[0085]

[0086] Comparing Example 4 and Example 5 with Example 1, Example 5 and Example 6 with Example 2, and Example 7 and Example 8 with Example 3, it was verified that the drying condition of the repair scheme is drying at 80 degrees for 4.5 hours. Under this condition, the mold material prepared has the best hardness and surface roughness.

[0087] Comparing Example 5 and Example 7 with Example 1, Example 4 and Example 8 with Example 2, and Example 5 and Example 6 with Example 3, it is verified that the mold material prepared under the preparation condition of sintering at 2100°C for 1 hour has the best hardness and surface roughness.

[0088] Based on this application, it should be understood by those skilled in the art that one aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.

[0089] It should be noted that the above embodiments can be freely combined as needed. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered as the protection scope of the present invention.

[0090] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as reference separately. In addition, it should be understood that after reading the above content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A graphite material mending agent for repairing a repairable forming mold, characterized in that: The graphite material repair agent comprises: In terms of mass percentage, silicon dioxide 30-70%, silica sand 10-30%, silica gel 5-20%, polyvinyl alcohol 5-15%, and graphite of the same mass as the total mass of these materials. The graphite material repair agent also includes hydrated sodium silicate, and the weight ratio of the hydrated sodium silicate to the silicon dioxide is between 1:1 and 1:

2.

2. The graphite material repair agent according to claim 1, characterized in that: The mass percentages of the silicon dioxide, silica sand, silica gel and polyvinyl alcohol components are between 50-70%, 15-25%, 5-15% and 5-15%.

3. The graphite material repair agent according to claim 1, characterized in that: The preparation method thereof comprises the following steps: mixing silicon dioxide, silica sand, silica gel and polyvinyl alcohol to obtain a suspension; The suspension is mixed with an equal mass of graphite to obtain the graphite material repair agent.

4. A method for repairing a forming mold, characterized in that: The steps include: Provide repairable forming dies; Providing the graphite material repair agent as claimed in claim 1; The repairable forming mold is repaired by using the graphite material repair agent and dried at 25-400° C., thereby achieving the reuse of the forming mold.

Citation Information

Patent Citations

  • Preparation method for die graphite material used for electrical discharge machining

    CN102898142A

  • Molding tool for molten metal or glass

    CN108290353A

  • High temperature oxidation-resistant graphite ceramic composite material and preparation method thereof

    CN109320246A

  • Graphite fireproof binder and preparation method

    CN109777305A

  • Mold repairing soft mud for casting, and preparation method thereof

    CN109912311A