Flame-retardant silicone tube for water and gas pipe and preparation method thereof
By using carbon nanotubes to graft organic molecules in silicone tubes, the problem of insufficient flame retardant performance of silicone tubes in high temperature and high humidity environments is solved, and its mechanical properties and flame retardant effect are improved, thus achieving It has better thermal insulation and oxygen resistance.
Patent Information
- Application Number
- CN202310387439.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-04-12
AI Technical Summary
Existing silicone tubes are difficult to withstand for a long time in high temperature and high humidity environments, and the flame retardant performance is insufficient, so they cannot effectively protect the inner tube and the liquid or gas circulating in the inner tube.
The flame retardant made of organic molecules modified by carbon nanotube grafting is adopted to introduce phosphorus and nitrogen elements to form a phosphorus-nitrogen system to improve the flame retardancy and mechanical properties of silicone tubes. By carboxylation of carbon nanotubes and SOCl2, The flame retardant is prepared by chemical reactions such as DMF, melamine, pyridine, etc., and mixed with silica gel, black masterbatch, reinforcement filler, and vulcanizing agent, and then extruded and vulcanized at high temperature.
It significantly improves the flame retardant and mechanical properties of silicone tubes, enhances its heat insulation and oxygen resistance capabilities at high temperatures, reduces the negative impact of flame retardant on its own performance, and improves strength, fatigue resistance and impact resistance. sex.
Smart Images

Figure BDA0004174515410000021 
Figure BDA0004174515410000022 
Figure BDA0004174515410000031
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicone processing, and in particular, relates to a flame-retardant silicone tube for a water and gas pipe and a preparation method thereof. Background Art
[0002] Silicone tubes can be wrapped around the outside of water pipes, gas pipes and other pipes to increase the strength and durability of the pipes. They are widely used in modern industry, defense industry and daily necessities.
[0003] When the silicone tube is used as a covering outer tube, it may be exposed to high temperature and high humidity environments, or even encounter fire during actual use. In order to protect the inner tube and the liquid, gas and other materials flowing in the inner tube, high requirements are placed on the flame retardant properties of the silicone tube. However, ordinary silicone tubes usually cannot withstand high temperatures for a long time. Therefore, it is necessary to improve the thermal stability and flame retardancy of the silicone tube to meet the durability requirements. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a flame retardant silicone tube for water and gas pipes and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A flame-retardant silicone tube for a water and gas pipe is made from the following raw materials in parts by weight: 100 parts of silicone, 2-3 parts of black masterbatch, 10-20 parts of reinforcing filler, 1.5-3 parts of vulcanizing agent, and 2-3 parts of flame retardant.
[0007] Furthermore, the silicone rubber used is methyl vinyl silicone rubber.
[0008] Furthermore, the reinforcing filler used is fumed silica.
[0009] Furthermore, the vulcanizing agent used is a di-tetra-vulcanizing agent.
[0010] Furthermore, the flame retardant is modified carbon nanotubes, which are prepared by the following steps:
[0011] S1. Add carboxylated carbon nanotubes into a flask, then add SOCl2 (thionyl chloride), ultrasonicate for 2 hours, then heat under reflux for 20 hours, then filter the reaction solution, vacuum dry the solid for 5 hours, then add DMF as solvent, then add melamine and pyridine, react at 80°C under nitrogen protection for 20 hours, then filter, wash the product with DMF and water in turn, and then vacuum dry for 10 hours to obtain intermediate 1; the ratio of carboxylated carbon nanotubes, SOCl2, melamine, and pyridine is 10g:100mL:22.1g:0.15mL;
[0012] The -COOH on the surface of the carboxylated carbon nanotubes is chlorinated by sulfoxide chloride, and then reacts with the -NH2 on melamine to obtain intermediate 2. The specific reaction process is as follows:
[0013]
[0014] S2, add intermediate 1 and glycolaldehyde into a flask, add ethanol and DMF, heat and reflux for 6h, after the reaction is completed, filter the reaction solution, wash the product with DMF and water in turn, and obtain intermediate 2; the ratio of intermediate 1, glycolaldehyde, ethanol, and DMF is 10g:7.2g:50mL:50mL;
[0015] The amino group of intermediate 1 and the aldehyde group on glycolaldehyde undergo condensation reaction to form a Schiff base to obtain intermediate 2. The specific reaction process is as follows:
[0016]
[0017] S3, intermediate 2 and dimethylphosphonyl chloride were placed in a flask, DMF and water were added, potassium carbonate was added in batches, the temperature was raised to 80°C for reaction for 6 hours, the reaction solution was filtered, and the product was washed with DMF and water in turn to obtain a flame retardant; the ratio of intermediate 2, dimethylphosphonyl chloride, DMF, water, and potassium carbonate was 10g:9.96g:75mL:25mL:8.28g;
[0018] Intermediate 2 and dimethylphosphonyl chloride are subjected to Williamson synthesis under alkaline conditions to generate ether to obtain a flame retardant. The specific reaction process is as follows:
[0019]
[0020] Flame retardant is made by grafting organic molecules with carbon nanotubes. The phosphorus and nitrogen elements introduced form a phosphorus-nitrogen system. Phosphide decomposes at high temperature to produce polymetaphosphoric acid. It is a very strong dehydrating agent, which can promote the carbonization of organic compounds to form a coke layer on the surface at high temperature, playing the role of heat insulation and oxygen barrier. Nitride plays the role of foaming agent and coke enhancer. In the combustion process, the non-combustible gases such as N2, CO2, H2O generated by thermal decomposition can also dilute the concentration of combustible gases.
[0021] Carbon nanotubes are interwoven into a network structure in the coke layer, which can improve the density and stability of the coke layer. As a nanomaterial, it has a high specific surface area and nano effect, which can make the particle size of the flame retardant smaller and achieve better flame retardant and smoke suppression effects. It can also reduce the amount of flame retardant used and reduce the adverse effects of the addition of flame retardants on the weakening of the performance of the silicone tube itself. At the same time, carbon nanotubes themselves have excellent mechanical properties, which can improve the strength, fatigue resistance and impact resistance of the silicone tube.
[0022] Further, the carboxylated carbon nanotubes are prepared by the following steps:
[0023] Place carbon nanotubes in a flask and add 10 mol / L nitric acid solution, ultrasonicate at room temperature for 1 hour, heat to 50°C and stir for 3 hours, centrifuge after the reaction, then wash with anhydrous ethanol until neutral, and vacuum dry at 60°C for 24 hours. Spread the oxidatively dried solid evenly on a watch glass, put it in a low-temperature plasma, introduce air, and treat it at 200W for 6 minutes to obtain carboxylated carbon nanotubes; the ratio of carbon nanotubes to nitric acid is 1g:100mL;
[0024] Nitric acid can oxidize carbon nanotubes, thereby introducing a certain number of carboxyl active groups on the side walls and tops of carbon nanotubes, providing reaction sites for carbon nanotube modification.
[0025] Another object of the present invention is to provide a method for preparing a flame-retardant silicone tube for a water and gas pipe, comprising the following steps;
[0026] In the first step, silica gel, black masterbatch, reinforcing filler, vulcanizing agent and flame retardant are added into an internal mixer for mixing to obtain a mixture;
[0027] In the second step, the kneaded mixture is passed through the extrusion die of an extrusion molding machine to obtain a molded silicone hose, which is then placed in a drying oven for high-temperature vulcanization, then wound into a roll, and subjected to secondary vulcanization at high temperature to obtain a flame-retardant silicone hose for water and gas pipes.
[0028] Beneficial effects of the present invention:
[0029] The present invention adds a flame retardant made by modifying carbon nanotubes grafted with organic molecules into the silicone tube, and the introduced phosphorus and nitrogen elements form a phosphorus-nitrogen system. The phosphide decomposes at high temperature to produce a coke layer, which plays a role of heat insulation and oxygen barrier. The nitride decomposes under heat during the combustion process to generate non-combustible gases such as N2, CO2, H2O, etc., which can dilute the concentration of combustible gases, thereby improving the flame retardancy of the silicone tube.
[0030] As a nanomaterial, carbon nanotubes can make the particle size of flame retardants smaller, achieving better flame retardant and smoke suppression effects. They can also reduce the amount of flame retardants used and reduce the adverse effects of the addition of flame retardants on the performance of silicone tubes themselves. At the same time, they can improve the strength, fatigue resistance and impact resistance of silicone tubes. DETAILED DESCRIPTION
[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] Preparation of carboxylated carbon nanotubes:
[0034] 10g of carbon nanotubes were placed in a flask and 1L of 10mol / L nitric acid solution was added. The mixture was ultrasonicated at room temperature for 1h, heated to 50℃ and stirred for 3h. After the reaction, the mixture was centrifuged, washed with anhydrous ethanol until neutral, and vacuum dried at 60℃ for 24h. The oxidatively dried solid was evenly spread on a watch glass, placed in a low-temperature plasma, air was introduced, and treated at 200W for 6min to obtain carboxylated carbon nanotubes.
[0035] Example 2
[0036] Preparation of flame retardant:
[0037] S1. Add 10 g of carboxylated carbon nanotubes into a flask, then add 100 mL of SOCl2 (sulfoxide chloride), ultrasonicate for 2 h, then heat under reflux for 20 h, then filter the reaction solution, vacuum dry the solid for 5 h, then add 22.1 g of melamine, 100 mL of DMF and 0.15 mL of pyridine, react at 80 ° C under nitrogen protection for 20 h, then filter, wash the product with DMF and water in turn, and then vacuum dry for 10 h to obtain intermediate 1;
[0038] S2, add 10g of intermediate 1 and 7.2g of glycolaldehyde into a flask, add 50mL of ethanol and 50mL of DMF, heat and reflux for 6h, after the reaction is completed, filter the reaction solution, wash the product with DMF and water in turn, to obtain intermediate 2;
[0039] S3. Put 10g of intermediate 2 and 9.96g of dimethylphosphonyl chloride into a flask, add 75mL of DMF and 25mL of water, add potassium carbonate in batches, raise the temperature to 80°C and react for 6h. After the reaction is completed, filter the reaction liquid, wash the product with DMF and water in turn to obtain a flame retardant.
[0040] Example 3
[0041] Preparation of flame retardant:
[0042] S1, add 20g of carboxylated carbon nanotubes into a flask, then add 200mL of SOCl2 (sulfoxide chloride), ultrasonicate for 2h, then heat under reflux for 20h, then filter the reaction solution, vacuum dry the solid for 5h, then add 44.2g of melamine, add 200mL of DMF and 0.3mL of pyridine, react at 80℃ under nitrogen protection for 20h, then filter, wash the product with DMF and water in turn, and then vacuum dry for 10h to obtain intermediate 1;
[0043] S2, add 20g of intermediate 1 and 14.4g of glycolaldehyde into a flask, add 100mL of ethanol and 100mL of DMF, heat and reflux for 6h, after the reaction is completed, filter the reaction solution, wash the product with DMF and water in turn, to obtain intermediate 2;
[0044] S3. Put 20g of intermediate 2 and 19.92g of dimethylphosphonyl chloride into a flask, add 150mL of DMF and 50mL of water, add potassium carbonate in batches, raise the temperature to 80°C and react for 6h. After the reaction is completed, filter the reaction liquid, wash the product with DMF and water in turn to obtain a flame retardant.
[0045] Example 4
[0046] 1000g of methyl vinyl silicone rubber, 20g of black masterbatch, 100g of fumed silica, 15g of di-tetra-vulcanizing agent and 20g of the flame retardant prepared in Example 2 are added to an internal mixer for mixing. The mixed mixture is passed through an extrusion die of an extrusion molding machine to obtain a molded silicone hose, which is then put into a drying oven for high-temperature vulcanization, then wound into a roll, and subjected to secondary vulcanization at high temperature to obtain a flame-retardant silicone hose for water and gas pipes.
[0047] Example 5
[0048] 1000g of methyl vinyl silicone rubber, 25g of black masterbatch, 150g of fumed silica, 22.5g of di-tetra-vulcanizing agent and 25g of the flame retardant prepared in Example 3 are added to an internal mixer for mixing. The mixed mixture is passed through an extrusion die of an extrusion molding machine to obtain a molded silicone hose, which is then put into a drying oven for high-temperature vulcanization, then wound into a roll, and subjected to secondary vulcanization at high temperature to obtain a flame-retardant silicone hose for water and gas pipes.
[0049] Example 6
[0050] 1000g of methyl vinyl silicone rubber, 30g of black masterbatch, 200g of fumed silica, 30g of di-tetra-vulcanizing agent and 30g of the flame retardant prepared in Example 2 are added to an internal mixer for mixing. The mixed mixture is passed through an extrusion die of an extrusion molding machine to obtain a molded silicone hose, which is then put into a drying oven, vulcanized at high temperature, and then wound into a roll, and secondary vulcanized at high temperature to obtain a flame-retardant silicone tube for water and gas pipes.
[0051] The flame-retardant silicone tube for water and gas pipes obtained in Examples 4-6 was subjected to the following performance tests: low-temperature elasticity was tested according to standard GB / T5564-94; bonding strength was tested according to standard GB532-1989; high-temperature resistance was tested according to standard GB / T3512-1983; flame retardancy was tested according to standard UL-94;
[0052]
[0053]
[0054] It can be seen from the data in the above table that by adding the flame retardant, the silicone tube obtained by the present invention has good mechanical properties and flame retardant properties.
[0055] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0056] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A flame-retardant silicone tube for water and gas pipes, characterized in that: It is made by mixing silica gel, black masterbatch, reinforcing filler, vulcanizer and flame retardant; Wherein, the flame retardant is prepared by the following steps: S1. Add carboxylated carbon nanotubes into a flask, then add SOCl2, ultrasonicate for 2h, then heat under reflux for 20h, then filter the reaction solution, vacuum dry the solid for 5h, then add DMF as solvent, then add melamine and pyridine, react at 80°C under nitrogen protection for 20h, then filter, wash the product with DMF and water in turn, and then vacuum dry for 10h to obtain intermediate 1; S2, adding intermediate 1 and glycolaldehyde into a flask, adding ethanol and DMF, heating and reflux for 6 hours, after the reaction is completed, filtering the reaction solution, washing the product with DMF and water in turn, to obtain intermediate 2; S3. Put intermediate 2 and dimethylphosphonyl chloride into a flask, add DMF and water, add potassium carbonate in batches, raise the temperature to 80°C and react for 6 hours, filter the reaction solution, wash the product with DMF and water in turn, and obtain a flame retardant.
2. The flame-retardant silicone tube for water and gas pipes according to claim 1, characterized in that: In step S1, the ratio of the amount of carboxylated carbon nanotubes, SOCl2, melamine, and pyridine is 10 g:100 mL:22.1 g:0.15 mL.
3. The flame-retardant silicone tube for water and gas pipes according to claim 1, characterized in that: In step S2, the ratio of the amount of intermediate 1, glycolaldehyde, ethanol and DMF is 10 g:7.2 g:50 mL:50 mL.
4. The flame-retardant silicone tube for water and gas pipes according to claim 1, characterized in that: In step S3, the ratio of the amount of intermediate 2, dimethylphosphonyl chloride, DMF, water and potassium carbonate is 10 g:9.96 g:75 mL:25 mL:8.28 g.
5. The flame-retardant silicone tube for water and gas pipes according to claim 1, characterized in that: The raw materials are calculated by weight as follows: 100 parts of silica gel, 2-3 parts of black masterbatch, 10-20 parts of reinforcing filler, 1.5-3 parts of vulcanizing agent, and 2-3 parts of flame retardant.
6. A method for preparing a flame-retardant silicone tube for water and gas pipes according to claim 1, characterized in that: The steps include: In the first step, silica gel, black masterbatch, reinforcing filler, vulcanizing agent and flame retardant are mixed to obtain a mixture; In the second step, the mixture is formed by extrusion, vulcanized at high temperature, then wound into a roll, and subjected to secondary vulcanization to obtain the silicone tube.