A method for preparing a composite alkali-activated building solid waste-based cementitious material and a building solid waste semi-rigid base

By stimulating the preparation of building solid waste-based gelling materials through composite alkali, the problem of low value-added utilization of construction solid waste is solved, high value-added utilization and environmentally friendly semi-rigid base preparation of building solid waste is achieved, and the strength of the material is improved. Economical applicability.

CN116514425BActive Publication Date: 2024-11-22CHANGSHA UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310496299.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-22
Estimated Expiration
2043-05-05

AI Technical Summary

Technical Problem

The low-value-added utilization of construction solid waste in road projects is not economically applicable, has not achieved high-value-added utilization, and the stacking and landfill lead to waste of resources and environmental pollution.

Method used

The preparation method of the compound alkali-activated construction solid waste-based gelling material includes picking, cleaning, crushing, calcining and activating construction solid waste, and mixing and stirring with a mixed solution of potassium hydroxide and potassium silicate as a composite alkali exciter, and adding Aluminate coupling agent and nanosilicon dioxide are used as composite activators to prepare high-strength semi-rigid base layers of construction solid waste.

Benefits of technology

It realizes the high value-added utilization of construction solid waste, reduces resource waste and environmental pollution, reduces carbon emissions and energy consumption, improves the activity and strength of materials, and is suitable for semi-rigid bases in road projects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116514425B_ABST
    Figure CN116514425B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a composite alkali-activated building solid waste-based cementitious material and a semi-rigid base layer of building solid waste. After picking out impurities in the building solid waste, the building solid waste is cleaned, dried, crushed, calcined and activated to obtain a building solid waste precursor material; a composite alkali-activated building solid waste-based cementitious material is obtained by weighing a composite alkali-activated building solid waste-based cementitious material according to 20 to 30% of the building solid waste precursor material, adding water and the building solid waste precursor material, and mixing and stirring to obtain the composite alkali-activated building solid waste-based cementitious material. The building solid waste is used as aggregate, and the building solid waste is modified to reduce the water absorption rate and crushing value of the building solid waste; the composite alkali-activated building solid waste-based cementitious material is added and mixed with the modified building solid waste aggregate to prepare a semi-rigid base layer, and the addition amount of the composite alkali-activated building solid waste-based cementitious material is 4 to 6% of the mass of the modified building solid waste aggregate, thereby realizing high added value utilization of building solid waste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of road engineering and relates to a preparation method of a composite alkali-activated construction solid waste-based cementitious material and a construction solid waste semi-rigid base layer. Background Art

[0002] With the continuous acceleration of urbanization in my country, a large number of municipal infrastructure construction and renovation projects have led to a sharp increase in the production of construction solid waste. Most of these construction solid wastes are transported to the suburbs for stacking or landfill without being treated, causing great waste of resources and environmental pollution. In the field of road engineering, processed construction solid waste is mainly used as roadbed filler or as recycled aggregate in the base or subbase of the road surface. However, although the use of construction solid waste as recycled aggregate in the base or subbase of the road surface can increase certain economic value, the high transportation cost still restricts the recycling rate of construction solid waste and its radiation range. Therefore, the use of construction solid waste as roadbed filler is only a low-value-added utilization and is not economically applicable under long transportation distances. If we want to improve the utilization rate of construction solid waste, the key lies in the development of high-value-added utilization technology for construction solid waste. Summary of the invention

[0003] The purpose of the embodiment of the present invention is to provide a method for preparing a composite alkali-activated construction solid waste-based cementitious material to solve the problem that the current low-value-added utilization of construction solid waste is not economically applicable and the high-value-added utilization of construction solid waste has not been achieved.

[0004] Another object of an embodiment of the present invention is to provide a method for preparing a semi-rigid base layer of construction solid waste.

[0005] The technical solution adopted in the embodiment of the present invention is: a method for preparing a composite alkali-activated construction solid waste-based cementitious material, which is carried out according to the following steps:

[0006] Step S1, after picking out impurities in the construction solid waste, the construction solid waste is washed, dried, crushed, calcined and activated to obtain a construction solid waste precursor material;

[0007] Step S2, weighing the composite alkali activator, adding water and the construction solid waste precursor material, and mixing and stirring to obtain the composite alkali-activated construction solid waste-based cementitious material.

[0008] Furthermore, the specific steps of step S1 are as follows:

[0009] Step S11, washing and drying the construction solid waste, the construction solid waste includes concrete, bricks, and tiles;

[0010] Step S12, crushing the construction solid waste into fine particles with a particle size of 3 to 20 mm, and then grinding the construction solid waste powder into a particle size of 100 to 200 μm;

[0011] Step S13, adding 6%-8% of the mass of the construction waste powder into the sodium hydroxide, calcining the mixture of the construction waste powder and the sodium hydroxide at 600-800° C. and then cooling;

[0012] Step S14, adding an activator to the calcined and cooled construction solid waste powder to obtain an activated construction solid waste material;

[0013] Step S15, crushing and ball-milling the activated construction solid waste material to a particle size of 10 to 20 μm to obtain a construction solid waste precursor material.

[0014] Furthermore, in step S12, the Si content of the construction solid waste powder is between 50% and 57%, the Al content is between 11% and 18%, and the Ca content is between 32% and 39%.

[0015] Furthermore, in step S14, 0.5-1% of aluminate coupling agent and 1-2% of nano silicon dioxide are added to the construction solid waste powder as a composite activator.

[0016] Furthermore, in step S2, a mixed solution of potassium hydroxide and potassium silicate is used as a composite alkali activator, the total content of K2O and SiO2 in the potassium silicate solution is above 35%, and the potassium hydroxide is a solid flake alkali with a purity of >98%.

[0017] Further, the amount of potassium hydroxide x to be added per 100g of potassium silicate solution is related to the target alkali activator modulus M x In accordance with formula (1):

[0018]

[0019] Where M x is the target base activator modulus, m s is the mass proportion of SiO2 in potassium silicate solution, M s is the relative molecular mass of SiO2, m n is the mass proportion of K2O in potassium silicate solution, M n is the relative molecular mass of K2O, M h is the relative molecular mass of KOH.

[0020] Furthermore, in step S2, a composite alkali activator with a modulus of 1.0 to 1.4 is weighed according to 20 to 30% of the construction solid waste precursor material, and water and the construction solid waste precursor material are added according to a water-cement ratio of 0.30 to 0.35, and mixed and stirred for 10 to 15 minutes to obtain a composite alkali-activated construction solid waste-based cementitious material.

[0021] Another technical solution adopted in the embodiment of the present invention is: a method for preparing a semi-rigid base layer of construction solid waste, using the composite alkali-activated construction solid waste-based cementitious material prepared as above, comprising the following steps:

[0022] Step 1: Using construction solid waste as aggregate, modifying the construction solid waste, and reducing the water absorption rate and crushing value of the construction solid waste;

[0023] Step 2: Add composite alkali-activated construction solid waste-based cementitious material and mix it with the modified construction solid waste aggregate to prepare a semi-rigid base layer.

[0024] Furthermore, in step 2, the amount of the composite alkali-activated construction solid waste-based cementitious material added is 4 to 6% of the mass of the modified construction solid waste aggregate.

[0025] Furthermore, the specific operations of step 1 are as follows:

[0026] Step 11, preparing ultrafine cement slurry, mixing 2-3% of the mass of aggregate with the ultrafine cement slurry and construction solid waste to strengthen the construction solid waste;

[0027] Step 12: After drying the construction solid waste reinforced with ultrafine cement, soak it in a silicone oil aqueous solution with a concentration of 3 to 5% by mass of aggregate for 18 to 24 hours.

[0028] The beneficial effects of the embodiments of the present invention are:

[0029] 1. Using construction solid waste to prepare composite alkali-activated construction solid waste-based cementitious materials, and using construction solid waste as aggregate and composite alkali-activated construction solid waste-based cementitious materials to prepare the entire construction solid waste semi-rigid base, not only solves the problem of resource waste and environmental pollution caused by large-scale stacking and landfilling of construction solid waste, but also realizes the high added value utilization of construction solid waste, and solves the problem that the current low added value utilization of construction solid waste is not economically applicable and has not achieved high added value utilization of construction solid waste;

[0030] 2. Using a mixture of potassium hydroxide and potassium silicate as a composite alkali activator is not easy to carbonize in the air. On the premise of achieving a good activating effect, the efflorescence phenomenon of composite alkali activating construction solid waste-based cementitious materials is reduced;

[0031] 3. Compared with traditional cementitious materials, the prepared composite alkali-activated construction solid waste-based cementitious materials rely on geopolymerization to generate gel products to form strength. The strength formation speed is fast, and no heat is released during geopolymerization. Replacing traditional cementitious materials such as cement and lime can reduce carbon emissions and energy consumption;

[0032] 4. The chemical composition of construction solid waste materials from different sources varies greatly. The embodiment of the present invention realizes the ratio control of chemical components based on the composition ratio of construction solid waste materials, thereby avoiding the influence of the difference in chemical composition of construction solid waste materials from different sources;

[0033] 5. The use of aluminate coupling agent and nano-silica as composite activators combined with high-temperature calcination of construction solid waste materials and sodium hydroxide significantly improves the activity of construction solid waste materials, allowing the construction solid waste materials to react more fully in the geopolymerization reaction and generate more products, thereby improving the strength of composite alkali-activated construction solid waste-based cementitious materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0035] Figure 1 It is a design drawing of the composition of each component in the precursor materials of construction solid waste.

[0036] Figure 2 yes Figure 1 The silicon, aluminum and calcium content diagram corresponding to each component design in the construction solid waste precursor material.

[0037] Figure 3 This is a real picture of the composite alkali-activated construction solid waste-based cementitious material specimen.

[0038] Figure 4 This is a diagram of the optimal ratio range of silicon, aluminum and calcium components in the construction solid waste precursor material according to an embodiment of the present invention. DETAILED DESCRIPTION

[0039] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] Example 1

[0041] The embodiment of the present invention provides a method for preparing a composite alkali-activated construction solid waste-based cementitious material, comprising the following steps:

[0042] Step S1: After picking out impurities from the construction solid waste, the construction solid waste is washed, dried, crushed, calcined, and activated to obtain a construction solid waste precursor material. The specific steps are as follows:

[0043] Step S11, washing and drying the construction solid waste, the construction solid waste comes from the demolition of buildings, and the main components include concrete, bricks, and tiles;

[0044] Step S12, crushing the construction solid waste into fine material with a particle size of 3 to 20 mm by a jaw crusher, and then crushing it into construction solid waste powder with a particle size of 100 to 200 μm by a pulverizer;

[0045] Step S13, adding 6-8% of the mass of the construction solid waste powder into the sodium hydroxide, calcining the construction solid waste powder and the sodium hydroxide mixture at 600-800° C. for 20-40 minutes and then cooling. The purpose of adding sodium hydroxide and the construction solid waste for calcining is to increase the content of amorphous substances (non-crystalline structure) in the construction solid waste, thereby stimulating the activity of the construction solid waste material;

[0046] Using 0.8% aluminate coupling agent, 1.5% nano-silica as composite activator, 7% sodium hydroxide dosage, water-cement ratio of 0.35, 25% alkali activator dosage and 1.0 alkali activator modulus, composite alkali-activated construction solid waste-based cementitious materials were prepared using construction solid waste powder after different calcination temperatures, and their 28d strength was tested. The results are shown in Table 1.

[0047] Table 1 Strength of composite alkali-activated building solid waste-based cementitious materials at different calcination temperatures

[0048]

[0049] Using 0.8% aluminate coupling agent and 1.5% nano-silica as composite activators, at a calcination temperature of 600°C, a calcination time of 40 min, a water-cement ratio of 0.35, an alkali activator dosage of 25% and an alkali activator modulus of 1.0, composite alkali-activated construction solid waste-based cementitious materials were prepared using construction solid waste powder with different sodium hydroxide dosages. The 28d strength was tested and the results are shown in Table 2.

[0050] Table 2 Strength of composite alkali activated building solid waste-based cementitious materials with different sodium hydroxide dosages

[0051] Sodium hydroxide dosage Cementitious material strength 0% 27.3MPa 6% 37.3MPa 7% 37.5MPa 8% 37.7MPa 10% 37.3MPa

[0052] Step S14, adding 0.5-1% of aluminate coupling agent and 1-2% of nano-silicon dioxide as a composite activator to the calcined and cooled construction solid waste powder to obtain a construction solid waste activated material, thereby further improving the activity of the construction solid waste powder;

[0053] After calcining at 600°C for 40 min, composite alkali-activated construction solid waste-based cementitious materials with different composite activator dosages were prepared under the conditions of 7% sodium hydroxide dosage, 0.35 water-cement ratio, 25% alkali activator dosage and 1.0 alkali activator modulus, and their 28d strength was tested. The results are shown in Table 3.

[0054] Table 3 Strength of composite alkali activated building solid waste-based cementitious materials with different composite activator dosages

[0055] Aluminate coupling agent dosage Nano-silicon dioxide dosage Cementitious material strength 0% 1.5% 33.2MPa 0.5% 1.5% 36.7MPa 0.8% 1.5% 37.5MPa 1% 1.5% 38.8MPa 1.2% 1.5% 39.1MPa 0.8% 0% 34.9MPa 0.8% 1% 37.2MPa 0.8% 2% 38.1MPa 0.8% 2.5% 38.4MPa 0.8% 3% 38.5MPa

[0056] Step S15, putting the activated construction solid waste material into a ball mill and milling it to a particle size of 10 to 20 μm to obtain a construction solid waste precursor material;

[0057] Step S2: weigh a composite alkali activator with a modulus of 1.0 to 1.4 according to 20 to 30% of the construction solid waste precursor material, add water and the construction solid waste precursor material according to a water-cement ratio of 0.30 to 0.35, mix and stir for 10 to 15 minutes, and obtain a composite alkali-activated construction solid waste-based cementitious material. The 28d strength of the composite alkali-activated construction solid waste-based cementitious material prepared under different water-cement ratios, 25% alkali activator dosage and 1.0 alkali activator modulus is shown in Table 4.

[0058] Table 4 Strength of composite alkali-activated construction solid waste-based cementitious materials at different water-cement ratios

[0059] Water-cement ratio Composite alkali activated cementitious materials based on construction solid waste 0.30 39.8MPa, poor fluidity 0.35 37.5MPa 0.40 33.4MPa, strength reduced 0.45 23.6MPa, low strength

[0060] The embodiment of the present invention adopts a mixed solution of potassium hydroxide and potassium silicate as a composite alkali activator. The total content of K2O and SiO2 in the potassium silicate solution is above 35%. Preferably, the potassium silicate solution contains 12.5% ​​K2O and 26.33% SiO2, and the original modulus is 3.3. Potassium hydroxide is a solid flake alkali with a purity of >98%. The modulus of the alkali activator refers to the molar ratio of K2O to SiO2 in the alkali activator. The modulus of the alkali activator will significantly affect the activating effect and thus affect the strength of the geopolymer. Adding potassium hydroxide is equivalent to adding K2O, and thus the modulus of the composite alkali activator of this embodiment can be adjusted. The embodiment of the present invention prepares the alkali activator according to the following steps:

[0061] The modulus of the alkali activator in the embodiment of the present invention is preferably 1.0 to 1.4. After calculation, the amount of potassium hydroxide x to be added per 100g of potassium silicate solution is proportional to the target modulus M of the alkali activator. x In accordance with formula (1):

[0062]

[0063] Where M x is the target base activator modulus, m sis the mass proportion of SiO2 in potassium silicate solution, M s is the relative molecular mass of SiO2, m n is the mass proportion of K2O in potassium silicate solution, M n is the relative molecular mass of K2O, M h is the relative molecular mass of KOH.

[0064] The mass of potassium hydroxide to be added is calculated according to the target modulus, and the potassium hydroxide is weighed and added to the potassium silicate solution, mixed and stirred for 5 to 10 minutes, and aged for 12 to 24 hours to obtain the composite alkali activator with the target modulus. Compared with conventional alkali activators, the composite alkali activator of the embodiment of the present invention reduces the efflorescence phenomenon of the gelling material while achieving a better activating effect.

[0065] Since the strength of geopolymers is related to the silicon, aluminum and calcium components in the precursor material, only the silicon, aluminum and calcium components in the construction solid waste are considered when designing the precursor material composition. Representative samples of each component of the construction solid waste were taken and the content of silicon, aluminum and calcium components was tested. The results are shown in Table 5.

[0066] Table 5 Silicon, aluminum and calcium content of each component of construction solid waste (%)

[0067] name Si Al Ca brick 52 15 4 ceramic tile 52 12 21 Concrete 30 6 48

[0068] The composition design of the three components of construction solid waste (bricks, tiles, and concrete) is carried out to control the content of silicon, aluminum, and calcium in the precursor materials of construction solid waste. Figures 1-2 As shown, Figure 1 Each intersection point corresponds to a material mix ratio. Figure 2 is the content of silicon, aluminum and calcium components corresponding to each mix ratio. According to the composition design, the mass of the precursor materials of each component was weighed to prepare the composite alkali-activated construction solid waste-based cementitious material. The composite alkali-activated construction solid waste-based cementitious material was poured into a 40×40×40mm cubic mold, vibrated for 2 to 3 minutes to remove bubbles, and cured for 28 days at a temperature of 23±3℃ and a relative humidity of more than 95%. The unconfined compressive strength test was performed. The composite alkali-activated construction solid waste-based cementitious material specimens were as follows: Figure 3 The test results are shown in Table 6.

[0069] Table 6 Unconfined compressive strength of composite alkali-activated building solid waste-based cementitious materials at 28 days

[0070] Serial number Concrete ceramic tile brick Strength (MPa) Serial number Concrete ceramic tile brick Strength (MPa) 1 0 0 1 34.6 34 0.2 0.5 0.3 37.3 2 0.1 0 0.9 36.9 35 0.1 0.6 0.3 34.3 3 0 0.1 0.9 33.5 36 0 0.7 0.3 32.8 4 0.2 0 0.8 37.6 37 0.8 0 0.2 38.9 5 0.1 0.1 0.8 35.5 38 0.7 0.1 0.2 39.2 6 0 0.2 0.8 32.1 39 0.6 0.2 0.2 38.1 7 0.3 0 0.7 39.3 40 0.5 0.3 0.2 38.8 8 0.2 0.1 0.7 38.3 41 0.4 0.4 0.2 41.2 9 0.1 0.2 0.7 34.1 42 0.3 0.5 0.2 38.4 10 0 0.3 0.7 31.1 43 0.2 0.6 0.2 37.1 11 0.4 0 0.6 37.8 44 0.1 0.7 0.2 35.7 12 0.3 0.1 0.6 36.8 45 0 0.8 0.2 32.9 13 0.2 0.2 0.6 32.6 46 0.9 0 0.1 38.2 14 0.1 0.3 0.6 29.6 47 0.8 0.1 0.1 39.1 15 0 0.4 0.6 27.8 48 0.7 0.2 0.1 39.5 16 0.5 0 0.5 43.4 49 0.6 0.3 0.1 38.2 17 0.4 0.1 0.5 38.7 50 0.5 0.4 0.1 37.4 18 0.3 0.2 0.5 31.4 51 0.4 0.5 0.1 40.5 19 0.2 0.3 0.5 28.4 52 0.3 0.6 0.1 40.9 20 0.1 0.4 0.5 26.6 53 0.2 0.7 0.1 36.4 21 0 0.5 0.5 23.1 54 0.1 0.8 0.1 32.6 22 0.6 0 0.4 39.7 55 0 0.9 0.1 31.7 23 0.5 0.1 0.4 42.9 56 1 0 0 36.2 24 0.4 0.2 0.4 38.6 57 0.9 0.1 0 36.1 25 0.3 0.3 0.4 36.4 58 0.8 0.2 0 35.4 26 0.2 0.4 0.4 36.2 59 0.7 0.3 0 36.7 27 0.1 0.5 0.4 35.8 60 0.6 0.4 0 37.8 28 0 0.6 0.4 32.3 61 0.5 0.5 0 38.6 29 0.7 0 0.3 38.2 62 0.4 0.6 0 40.2 30 0.6 0.1 0.3 39.1 63 0.3 0.7 0 39.2 31 0.5 0.2 0.3 42.2 64 0.2 0.8 0 37.1 32 0.4 0.3 0.3 41.8 65 0.1 0.9 0 34.2 33 0.3 0.4 0.3 38.2 66 0 1 0 32.4

[0071] The proportion of composite alkali-activated construction solid waste-based cementitious materials with unconfined compressive strength above 40 MPa was screened out, and the results were compared with those in Table 5, Table 6 and Figure 4In the construction solid waste powder, the Si content is between 50% and 57%, the Al content is between 11% and 18%, and the Ca content is between 32% and 39%. Figure 4 The overlapping triangle area in is the optimal ratio area of ​​the construction solid waste precursor material. When the silicon, aluminum and calcium content of the construction solid waste powder meets the requirements of this range, a high-strength composite alkali-activated construction solid waste-based cementitious material is obtained. When using different construction solid wastes to prepare composite alkali-activated construction solid waste-based cementitious materials, the ratio of each component of the construction solid waste (bricks, tiles, concrete) can be determined according to the silicon, aluminum and calcium content of each component.

[0072] Example 2

[0073] The embodiment of the present invention provides a method for preparing a semi-rigid base layer of construction solid waste, comprising the following steps:

[0074] Step 1: Use construction solid waste as aggregate to modify the construction solid waste and reduce the water absorption rate and crushing value of the construction solid waste. The specific operations are as follows:

[0075] Step 11, preparing ultrafine cement slurry according to a water-cement ratio of 0.45, mixing 2-3% of the mass of the aggregate with the construction solid waste to strengthen the construction solid waste, so that the ultrafine cement slurry is completely coated on the surface of the construction solid waste, blocking the fine pores of the construction solid waste, reducing the crushing value of the construction solid waste, and improving the strength of the construction solid waste. At a water-cement ratio of 0.45, the ultrafine cement slurry can be well mixed with the aggregate and coated on the aggregate, and the coating is uneven when the water-cement ratio is too high or too low;

[0076] Step 12, after drying the construction solid waste reinforced with ultrafine cement, soak it in a silicone oil aqueous solution with a concentration of 3 to 5% by mass of aggregate for 18 to 24 hours to reduce the water absorption rate of the construction solid waste;

[0077] Step 2: Mix the composite alkali-activated construction solid waste-based cementitious material of Example 1 with the modified construction solid waste aggregate at 4-6% of the modified construction solid waste aggregate to prepare a semi-rigid base layer.

[0078] The modified construction solid waste was subjected to a vibration compaction test to determine the optimal moisture content and maximum dry density of the modified construction solid waste. The compaction test results showed that the optimal moisture content was 7.2% and the maximum dry density was 2.323 g / cm 3The composite alkali-activated construction solid waste-based cementitious material was prepared by using the optimal ratio of concrete: tile: brick = 0.5: 0: 0.5, corresponding to silicon: aluminum: calcium = 53%: 14%: 33%. The composite alkali-activated construction solid waste-based cementitious material was mixed with the modified construction solid waste aggregate at a dosage of 4-6%. The semi-rigid base specimens were formed by the standard vibration compaction method in the specification based on the optimal moisture content and maximum dry density of the construction solid waste. The unconfined compressive strength test was carried out after curing for 7 days under the standard curing conditions in the specification (23±3℃, 95% relative humidity). The results are shown in Table 7.

[0079] Table 7 7d unconfined compressive strength test results of semi-rigid base specimens

[0080]

[0081]

[0082] It can be seen from Table 7 that the 7d unconfined compressive strength test results of the semi-rigid base specimens meet the strength requirements of the base for extremely heavy and extra-heavy traffic on expressways and first-class highways: the 7d unconfined compressive strength is 5.0-7.0MPa.

[0083] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.

Claims

1. A method for preparing a composite alkali-activated building solid waste-based cementitious material, characterized in that: Follow these steps: Step S1, after picking out impurities in the construction solid waste, the construction solid waste is washed, dried, crushed, calcined and activated to obtain a construction solid waste precursor material; Step S11, washing and drying the construction solid waste, the construction solid waste includes concrete, bricks, and tiles; Step S12, crushing the construction solid waste into fine particles with a particle size of 3 to 20 mm, and then grinding the construction solid waste powder into a particle size of 100 to 200 μm; Step S13, adding 6% to 8% of the mass of the construction waste powder into the sodium hydroxide, calcining the construction waste powder and the sodium hydroxide mixture at 600 to 800° C. for 20 to 40 minutes, and then cooling; Step S14, adding an activator to the calcined and cooled construction solid waste powder to obtain a construction solid waste activated material; 0.5-1% of the mass of the construction solid waste powder is an aluminate coupling agent and 1-2% of nano silicon dioxide is used as the activator; Step S15, crushing and ball-milling the activated construction solid waste material to a particle size of 10 to 20 μm to obtain a construction solid waste precursor material; Step S2, weighing a composite alkali activator, adding water and the construction solid waste precursor material, and mixing and stirring to obtain a composite alkali-activated construction solid waste-based gelling material; In step S12, the Si mass content of the construction solid waste powder is between 50 and 57%, the Al mass content is between 11 and 18%, and the Ca mass content is between 32 and 39%; In step S2, a mixed solution of potassium hydroxide and potassium silicate is used as a composite alkali activator, the total mass content of K2O and SiO2 in the potassium silicate solution is above 35%, and the potassium hydroxide is a solid flake alkali with a purity of >98%; The amount of potassium hydroxide x that needs to be added per 100g of potassium silicate solution is related to the target alkali activator modulus M x In accordance with formula (1): Where M x is the target base activator modulus, m s is the mass proportion of SiO2 in potassium silicate solution, M s is the relative molecular mass of SiO2, m n is the mass proportion of K2O in potassium silicate solution, M n is the relative molecular mass of K2O, M h is the relative molecular mass of KOH; In step S2, a composite alkali activator with a modulus of 1.0 to 1.4 is weighed according to 20 to 30% of the mass of the construction solid waste precursor material, and water and the construction solid waste precursor material are added according to a water-cement ratio of 0.30 to 0.35, and mixed and stirred for 10 to 15 minutes.

2. A method for preparing a semi-rigid base layer of construction solid waste, characterized in that: The composite alkali-activated construction solid waste-based cementitious material prepared according to claim 1 comprises the following steps: Step 1: Using construction solid waste as aggregate, modifying the construction solid waste, and reducing the water absorption rate and crushing value of the construction solid waste; Step 2: Add composite alkali-activated construction solid waste-based cementitious material and mix it with the modified construction solid waste aggregate to prepare a semi-rigid base layer.

3. The method for preparing a semi-rigid base layer of construction solid waste according to claim 2, characterized in that: In step 2, the amount of composite alkali-activated construction solid waste-based cementitious material added is 4-6% of the mass of the modified construction solid waste aggregate.

4. The method for preparing a semi-rigid base layer of construction solid waste according to claim 2, characterized in that: The specific operations of step 1 are as follows: Step 11, preparing ultrafine cement slurry, mixing 2-3% of the mass of aggregate with the ultrafine cement slurry and construction solid waste to strengthen the construction solid waste; Step 12: After drying the construction solid waste reinforced with ultrafine cement, soak it in a silicone oil aqueous solution with a concentration of 3 to 5% by mass of aggregate for 18 to 24 hours.