Modification method of bamboo aggregate and use of composition
By using ammonia-soluble quaternary ammonium copper and polyacrylate treatment in bamboo aggregates, a flexible adhesive layer is formed, which solves the corrosion problem of bamboo aggregates in alkaline environments, significantly improves its durability and compressive strength, and achieves the Higher corrosion resistance and alkali resistance.
Patent Information
- Application Number
- CN202310602462.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-05-26
AI Technical Summary
Bamboo aggregates are easily corroded and degraded in alkaline environments, affecting their durability and strength. The existing modification methods can only cross-link on the surface, and their durability and compressive strength are limited.
Soak bamboo aggregate in ammonia-soluble quaternary ammonium copper solution for 1 to 4 hours, and then soak in polyacrylate mixture for 12 to 24 hours. By forming a flexible adhesive layer, it can prevent alkaline corrosion and improve corrosion resistance and alkali resistance. sex.
It significantly improves the corrosion resistance and alkali resistance of bamboo aggregates, extends its service life, maintains mechanical properties and volume stability, and enhances the overall strength and durability of bamboo aggregate cement concrete.
Smart Images

Figure BDA0004249509070000071 
Figure BDA0004249509070000072 
Figure BDA0004249509070000081
Abstract
Description
Technical Field
[0001] The invention relates to a bamboo aggregate modification method and application of the composition. Background Art
[0002] At present, bamboo aggregate cement concrete, as a new type of bio-based renewable cement concrete material, has attracted more and more attention due to its light weight, low carbon and environmental protection. There are many problems in the use of bamboo aggregate in cement concrete. First, as an organic matter, bamboo is easily decomposed by various decay fungi, which reduces the strength of the bamboo aggregate itself and affects the durability of bamboo aggregate cement concrete. Secondly, the pH value of cement concrete in an alkaline environment can reach 12-14; in an alkaline environment, the cellulose, hemicellulose and lignin in the bamboo particles will dissolve, thereby seriously reducing the integrity and strength of the bamboo aggregate itself. Under the influence of the above unfavorable factors, the promotion and use of bamboo aggregate cement concrete has been seriously affected.
[0003] CN113563000A discloses a modified preparation method of bamboo aggregate and its application, wherein bamboo is used as the main raw material, chopped into bamboo particles, vibrated and screened, and then the bamboo particles are successively boiled, washed, soaked in sodium alginate solution, soaked in calcium chloride solution and dried to prepare a bamboo aggregate that can be used in the field of construction. However, since the polymers produced by cross-linking sodium alginate and calcium chloride are only wrapped on the surface of the bamboo aggregate particles, this method can only improve the corrosion resistance and alkali resistance of the bamboo aggregate to a certain extent, but the durability is poor and its compressive strength is also limited. Summary of the invention
[0004] In view of this, one object of the present invention is to provide a bamboo aggregate modification method, which can improve the corrosion resistance and alkali resistance of the bamboo aggregate. Another object of the present invention is to provide a composition for improving the corrosion resistance and alkali resistance of bamboo aggregate.
[0005] The present invention adopts the following technical solutions to achieve the above-mentioned purpose.
[0006] In one aspect, the present invention provides a method for modifying bamboo aggregate, comprising the following steps:
[0007] (1) soaking bamboo aggregate in ammonia-dissolved quaternary ammonium copper solution for 1 to 4 hours, and then ventilating and drying; wherein the weight ratio of the bamboo aggregate to the ammonia-dissolved quaternary ammonium copper solution is 1:2 to 3.5;
[0008] (2) Soaking the bamboo aggregates soaked in the ammonia-dissolved quaternary ammonium copper solution in a polyacrylate mixed solution for 12 to 24 hours, and then ventilating and drying to obtain modified bamboo aggregates; wherein the polyacrylate mixed solution is prepared by mixing a polyacrylate emulsion and water; and the weight ratio of the bamboo aggregates soaked in the ammonia-dissolved quaternary ammonium copper solution to the polyacrylate mixed solution is 1:2 to 3.5.
[0009] In step (1) of the present invention, the bamboo aggregate is soaked in an ammonia-soluble quaternary ammonium copper solution, which can improve the corrosion resistance of the bamboo aggregate. The weight ratio of the bamboo aggregate to the ammonia-soluble quaternary ammonium copper solution can be 1:2-3.5, preferably 1:2.5-3.1. The bamboo aggregate can be a pretreated bamboo aggregate, and the pretreatment process can include crushing, screening and drying the mature bamboo. In some embodiments, the mature bamboo can be crushed and screened to obtain wet bamboo aggregate, which is then soaked in an ammonia-soluble quaternary ammonium copper solution, and the soaking time can be 1-4 hours, preferably 2-4 hours. In other embodiments, the mature bamboo can be crushed, screened and then dried to obtain dry bamboo aggregate, which is then soaked in an ammonia-soluble quaternary ammonium copper solution, and the soaking time can be 1-2 hours, preferably 1-1.5 hours. Many existing wood preservatives are not only highly toxic and environmentally unfriendly, but may also change the mechanical properties of bamboo aggregates themselves. The inventors have found that ammonia-soluble quaternary ammonium copper is not only relatively environmentally friendly, but also can keep bamboo aggregates from rotting all year round after being soaked in ammonia-soluble quaternary ammonium copper solution, while not changing the mechanical properties of the bamboo aggregates themselves and enhancing the volume stability of the bamboo aggregates.
[0010] According to the method of the present invention, preferably, in step (1), the bamboo aggregate is pretreated bamboo aggregate, and the pretreatment comprises the following steps:
[0011] The mature bamboo is crushed into bamboo particles, and then the particles are vibrated and screened to obtain bamboo aggregate raw materials with a length of 5 to 15 mm, a width of 5 to 10 mm, and a thickness of 2 to 3 mm; the bamboo aggregate raw materials are then ventilated and dried at 65 to 85°C to obtain bamboo aggregate. The selected bamboo can be 3 to 5 years old. The pre-treated bamboo aggregate is more conducive to subsequent modification.
[0012] According to the method of the present invention, preferably, in step (1), the soaking time is 1 to 1.5 hours.
[0013] According to the method of the present invention, preferably, in step (1), the weight ratio of the ammonia-soluble quaternary ammonium copper to water in the ammonia-soluble quaternary ammonium copper solution is 1:7.5 to 15. More preferably, the weight ratio of the ammonia-soluble quaternary ammonium copper to water in the ammonia-soluble quaternary ammonium copper solution is 1:10 to 15.
[0014] According to the method of the present invention, preferably, in step (1), the drying temperature is 30-40° C. More preferably, the drying temperature is 33-36° C.
[0015] In step (2) of the present invention, the bamboo aggregates soaked in the ammonia-dissolved quaternary ammonium copper solution are soaked in a polyacrylate mixture, which can improve the alkali resistance of the bamboo aggregates. The weight ratio of the bamboo aggregates soaked in the ammonia-dissolved quaternary ammonium copper solution to the polyacrylate mixture can be 1:2-3.5, preferably 2.5-3.1. The inventor unexpectedly found that after the bamboo aggregates were soaked in the polyacrylate mixture, a flexible adhesion layer was formed in the pores of the vascular bundles and basic tissues of the bamboo aggregates, preventing the alkaline corrosion of the cement matrix alkalinity on the cell walls of the bamboo aggregates. Thereby improving the overall strength and durability of the bamboo aggregate cement concrete.
[0016] According to the method of the present invention, preferably, in step (2), the soaking time is 12 to 15 hours.
[0017] According to the method of the present invention, preferably, in step (2), the weight ratio of the polyacrylate emulsion to water in the polyacrylate mixed solution is 1:8 to 15. More preferably, the weight ratio of the polyacrylate emulsion to water in the polyacrylate mixed solution is 1:8 to 10.
[0018] According to the method of the present invention, preferably, in step (2), the drying temperature is 30-40°C; more preferably, the drying temperature is 33-36°C.
[0019] According to the method of the present invention, preferably, the moisture content of the bamboo aggregate soaked in the ammonia-dissolved quaternary ammonium copper solution in step (1) and the modified bamboo aggregate in step (2) is 7-13%.
[0020] According to one embodiment of the present invention, a method for modifying bamboo aggregate comprises the following steps:
[0021] (1) crushing mature bamboo into bamboo particles, and then vibrating and sieving through a screen to obtain bamboo aggregate raw materials with a particle size of 5 to 15 mm in length, 5 to 10 mm in width, and 2 to 3 mm in thickness; and then drying the bamboo aggregate raw materials at 65 to 85° C. through ventilation to obtain bamboo aggregate;
[0022] (2) soaking the bamboo aggregate in an ammonia-soluble quaternary ammonium copper solution for 1 to 4 hours, and then ventilating and drying the bamboo aggregate; wherein the weight ratio of the bamboo aggregate to the ammonia-soluble quaternary ammonium copper solution is 1:2 to 3.5;
[0023] (3) Soaking the bamboo aggregates soaked in the ammonia-dissolved quaternary ammonium copper solution in a polyacrylate mixed solution for 12 to 24 hours, and then ventilating and drying to obtain modified bamboo aggregates; wherein the polyacrylate mixed solution is prepared by mixing a polyacrylate emulsion and water; and the weight ratio of the bamboo aggregates soaked in the ammonia-dissolved quaternary ammonium copper solution to the polyacrylate mixed solution is 1:2 to 3.5.
[0024] On the other hand, the present invention also provides a use of a composition for improving the corrosion resistance and alkali resistance of bamboo aggregate, characterized in that the composition is ammonia-soluble quaternary ammonium copper and polyacrylate emulsion, comprising the following steps:
[0025] (1) soaking bamboo aggregate in ammonia-dissolved quaternary ammonium copper solution for 1 to 4 hours, and then ventilating and drying; wherein the weight ratio of the bamboo aggregate to the ammonia-dissolved quaternary ammonium copper solution is 1:2 to 3.5;
[0026] (2) Soaking the bamboo aggregates soaked in the ammonia-dissolved quaternary ammonium copper solution in a polyacrylate mixed solution for 12 to 24 hours, and then ventilating and drying to obtain modified bamboo aggregates; wherein the polyacrylate mixed solution is prepared by mixing a polyacrylate emulsion and water; and the weight ratio of the bamboo aggregates soaked in the ammonia-dissolved quaternary ammonium copper solution to the polyacrylate mixed solution is 1:2 to 3.5.
[0027] The method of the invention can effectively improve the corrosion resistance and alkali resistance of the bamboo aggregate, further improve the durability, and has simple steps and is easy to operate. DETAILED DESCRIPTION
[0028] The raw materials used in the embodiments and comparative examples are described below:
[0029] Ammonia-soluble quaternary ammonium copper (ACQ) was purchased from Dongguan Miaoqing Technology Co., Ltd., model MQKJ-651.
[0030] Polyacrylate emulsion, purchased from Beijing Mengtai Weiye Building Materials Co., Ltd., model MT 1068, solid content 55%.
[0031] Example 1
[0032] (1) crushing mature bamboo into bamboo particles, and then vibrating and sieving through a sieve to obtain bamboo aggregate raw materials with a particle size of 5 to 15 mm in length, 5 to 10 mm in width, and 2 to 3 mm in thickness; and then drying the bamboo aggregate raw materials at 70° C. by ventilation to obtain bamboo aggregate;
[0033] (2) Soaking the bamboo aggregate in an ammonia-dissolved quaternary ammonium copper solution (the weight ratio of the ammonia-dissolved quaternary ammonium copper to water is 1:15) for 1 hour, and then drying the bamboo aggregate under ventilation at 35°C; wherein the weight ratio of the bamboo aggregate to the ammonia-dissolved quaternary ammonium copper solution is 1:3;
[0034] (3) The bamboo aggregates soaked in the ammonia-soluble quaternary ammonium copper solution are soaked in a polyacrylate mixed solution (the weight ratio of the polyacrylate emulsion to water is 1:10) for 12 hours, and then ventilated and dried at 35°C to obtain modified bamboo aggregates; wherein the weight ratio of the bamboo aggregates soaked in the ammonia-soluble quaternary ammonium copper solution to the polyacrylate mixed solution is 1:3.
[0035] Comparative Example 1
[0036] The difference from Example 1 is that only step (1) is performed, and steps (2) and (3) are not performed. The properties of the obtained bamboo aggregate are shown in Table 1.
[0037] Comparative Example 2
[0038] The difference from Example 1 is that only steps (1) and (2) are performed, and step (3) is not performed. The properties of the obtained modified bamboo aggregate are shown in Table 1.
[0039] Comparative Example 3
[0040] The difference from Example 1 is that step (2) is not performed, and the bamboo aggregate obtained in step (1) is directly immersed in the polyacrylate mixed solution.
[0041] Comparative Example 4
[0042] The method in Example 5 of the prior art CN113563000A is used to modify bamboo aggregate, and compressive strength, mildew resistance and alkali resistance tests are carried out according to the test method of the present invention.
[0043] Experimental example
[0044] <Compressive strength and mildew resistance test>
[0045] The bamboo aggregates or modified bamboo aggregates of Example 1 and Comparative Examples 1 to 4 were prepared into bamboo aggregate cement concrete test blocks for strength and mildew resistance tests. The test steps are as follows:
[0046] Ingredients: Weigh the ingredients according to the mass ratio of cement: water: sand: bamboo aggregate or modified bamboo aggregate = 1:0.5:1.24:0.66.
[0047] First, add 10wt% of calcium chloride coagulant to water, mix it with cement, then add sand and stir evenly, finally add bamboo aggregate or modified bamboo aggregate to mortar and stir evenly, put it into a cubic mold with a side length of 100mm×100mm×100mm and vibrate it with a surface vibrator, cure it at room temperature for 24 hours, demould it, and put it in a standard curing room for 28 days to obtain a bamboo aggregate cement concrete test block. Then, the bamboo aggregate cement concrete test block is subjected to compressive strength test and mildew resistance test. Among them,
[0048] Compressive strength test
[0049] The compressive strength test was carried out according to GB / T 50081-2002 standard for test methods of mechanical properties of ordinary concrete.
[0050] Mildew resistance test
[0051] The bamboo aggregate cement concrete test blocks were directly placed outdoors for natural mildew, and the mildew condition was observed for 100 days.
[0052] The test results are shown in Table 1.
[0053] Table 1
[0054]
[0055] <Alkali resistance test>
[0056] Three portions of the modified bamboo aggregate obtained in Example 1 were weighed and recorded as A1, A2 and A3 as samples to be tested, wherein the mass of A1 was 300 g, the mass of A2 was 400 g, and the mass of A3 was 500 g. Three portions of the modified bamboo aggregate obtained in Comparative Example 4 were weighed and recorded as B1, B2 and B3 as samples to be tested, wherein the mass of B1 was 300 g, the mass of B2 was 400 g, and the mass of B3 was 500 g.
[0057] The test sample was placed in a saturated calcium hydroxide solution and soaked for 8h, 16h, 24h, 32h, 40h and 48h respectively, then taken out, washed and dried to constant weight, and finally the bamboo aggregate after drying was weighed and compared with the initial mass, and the mass change rate was calculated. The results are shown in Table 2. Among them, M1 represents the mass of the modified bamboo aggregate obtained in Comparative Example 4 after soaking in a saturated calcium hydroxide solution, and M2 represents the mass of the modified bamboo aggregate obtained in Example 1 after soaking in a saturated calcium hydroxide solution.
[0058] Table 2
[0059]
[0060]
[0061] It can be seen from Table 1 that the bamboo aggregate modified by the method of the present invention is superior to other comparative examples in terms of compressive strength and mildew resistance (corrosion resistance).
[0062] As can be seen from Table 2, the alkali resistance of the bamboo aggregate modified by the prior art method is weak, and accordingly, the durability is very limited. The mass change rate of the bamboo aggregate modified by the method of the present invention is significantly lower than that in the prior art, indicating that the degree of mass change is small, and further, the ability to resist alkaline degradation in an alkaline environment is strong.
[0063] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.
Claims
1. A method for modifying bamboo aggregate, characterized in that: The steps include: (1) soaking bamboo aggregate in ammonia-dissolved quaternary ammonium copper solution for 1 to 4 hours, and then ventilating and drying; wherein the weight ratio of the bamboo aggregate to the ammonia-dissolved quaternary ammonium copper solution is 1:2 to 3.5; (2) Soaking the bamboo aggregates soaked in the ammonia-dissolved quaternary ammonium copper solution in a polyacrylate mixed solution for 12 to 24 hours, and then ventilating and drying to obtain modified bamboo aggregates; wherein the polyacrylate mixed solution is prepared by mixing a polyacrylate emulsion and water; and the weight ratio of the bamboo aggregates soaked in the ammonia-dissolved quaternary ammonium copper solution to the polyacrylate mixed solution is 1:2 to 3.
5.
2. The method according to claim 1, characterized in that In step (1), the bamboo aggregate is pretreated bamboo aggregate, and the pretreatment comprises the following steps: The mature bamboo is crushed into bamboo particles, and then the particles are vibrated and sieved through a sieve to obtain bamboo aggregate raw materials with a length of 5-15 mm, a width of 5-10 mm, and a thickness of 2-3 mm; the bamboo aggregate raw materials are then ventilated and dried at 65-85° C. to obtain bamboo aggregate.
3. The method according to claim 2, characterized in that In step (1), the soaking time is 1 to 1.5 hours.
4. The method according to claim 3, characterized in that In step (1), the weight ratio of ammonia-soluble quaternary ammonium copper to water in the ammonia-soluble quaternary ammonium copper solution is 1:7.5-15.
5. The method according to claim 1, characterized in that In step (1), the drying temperature is 30-40°C.
6. The method according to claim 1, characterized in that In step (2), the soaking time is 12 to 15 hours.
7. The method according to claim 6, characterized in that In step (2), the weight ratio of the polyacrylate emulsion to water in the polyacrylate mixed solution is 1:8-15.
8. The method according to claim 1, characterized in that In step (2), the drying temperature is 30-40°C.
9. The method according to claim 1, characterized in that: The moisture content of the bamboo aggregate and the modified bamboo aggregate after being soaked in the ammonia-dissolved quaternary ammonium copper solution in step (2) is 7-13%.
10. Use of a composition for improving the corrosion resistance and alkali resistance of bamboo aggregate, characterized in that: The composition is ammonia-soluble quaternary ammonium copper and polyacrylate emulsion, comprising the following steps: (1) soaking bamboo aggregate in ammonia-dissolved quaternary ammonium copper solution for 1 to 4 hours, and then ventilating and drying; wherein the weight ratio of the bamboo aggregate to the ammonia-dissolved quaternary ammonium copper solution is 1:2 to 3.5; (2) Soaking the bamboo aggregates soaked in the ammonia-dissolved quaternary ammonium copper solution in a polyacrylate mixed solution for 12 to 24 hours, and then ventilating and drying to obtain modified bamboo aggregates; wherein the polyacrylate mixed solution is prepared by mixing a polyacrylate emulsion and water; and the weight ratio of the bamboo aggregates soaked in the ammonia-dissolved quaternary ammonium copper solution to the polyacrylate mixed solution is 1:2 to 3.5.