Industrial solid waste-based water-prevention grouting material and preparation method and use method thereof
By combining industrial solid waste-based water control grouting materials, the stability and early strength issues of cement-based materials have been resolved, achieving efficient and economical grouting results and promoting the comprehensive utilization of industrial solid waste.
Patent Information
- Application Number
- CN202310388311.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-04-12
AI Technical Summary
Existing water-control grouting materials, such as cement-based materials, suffer from poor stability, low early strength, long setting time, and high cost. They also have difficulty effectively utilizing industrial solid waste, resulting in high grouting costs and insufficient performance.
The grouting material for water control based on industrial solid waste is adopted, including phosphoaluminate cement clinker, granulated blast furnace slag, coal gangue, activated gypsum, nano-calcium carbonate, modified quicklime, and polymer emulsion. Through synergistic effect, a network crystal is generated, which improves the early strength and interfacial bonding strength. The network film formed by the polymer emulsion enhances the impermeability and flexural strength.
It significantly improves the stability and early strength of the stone body, shortens the setting time, reduces cement usage, lowers grouting costs, and realizes the comprehensive utilization of industrial solid waste, resulting in high economic and environmental benefits.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the field of comprehensive utilization of industrial solid waste and mine water prevention and control technology, and in particular to an industrial solid waste-based water prevention and control grouting material and a preparation method and a use method thereof. Background Art
[0002] Granulated blast furnace slag is an industrial waste slag with calcium silicate as the main component produced in the ironmaking process of steel plants. It has potential hydraulic cementitiousness and a huge output. Coal gangue, as solid waste produced in coal mining and coal preparation, is an inevitable product of coal mining and processing. It has prominent problems such as large quantity, large land area, and low comprehensive utilization efficiency. From the perspectives of effective utilization of resources, energy conservation and environmental protection, how to treat a large amount of industrial solid waste in a high-value manner has attracted the attention of more and more people.
[0003] The water prevention and control grouting reinforcement technology is to arrange drilling holes on the ground far away from the mining area before mining, to clearly explore the water-rich conditions and existing cracks in the coal seam floor rock, and use high-pressure grouting to press the grouting slurry into the cracks to seal the cracks and cut off the passage of lower groundwater to the coal seam, thereby preventing water damage during mining. At present, most of the grouting materials used in coal mine water prevention and control grouting projects are mainly cement. Although cement has the advantages of high strength, good durability, non-toxicity and tastelessness, and a wide range of material sources, cement as a grouting material will have the following problems: (1) The water-cement ratio of cement is large, which can easily lead to poor stability of the grouting material. At the same time, cement also has poor impermeability and toughness. After hardening, the solid phase volume shrinks and forms new water channels; (2) The stone body formed by cement has low adhesion and bonding with the rock matrix; (3) Cement has a long setting time in a water-rich state, low early strength, low water prevention and control efficiency, and high material consumption. Therefore, it is necessary to develop a grouting material with high stone body stability, high early strength, fast setting speed and economic applicability. Summary of the invention
[0004] In view of the problems of low industrial solid waste addition, poor stone body stability, low early strength, long setting time and high production cost in cement-based grouting materials in the prior art, the present invention provides an industrial solid waste-based water-preventive grouting material and a preparation method and a use method thereof.
[0005] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0006] An industrial solid waste-based water grouting material for prevention and control, comprising the following raw material components in parts by weight: 5-10 parts of phosphate aluminate cement clinker, 40-60 parts of granulated blast furnace slag, 20-30 parts of coal gangue, 3-10 parts of active gypsum, 2-5 parts of nano calcium carbonate, 3-10 parts of polymer emulsion, 4-10 parts of modified lime and 0.1-0.5 parts of composite admixture;
[0007] Wherein, the polymer emulsion comprises tetrahydrofurfuryl acrylate polymer modified polyacrylate emulsion and styrene-acrylic acid copolymer.
[0008] Most of the existing water prevention and control grouting materials are based on cement, and the amount of grouting materials used is large and the cost is high. The annual investment in water prevention and control grouting is tens of millions. In order to reduce the cost of grouting materials, people try to use a small amount of industrial waste residue, such as coal gangue, slag, etc. However, in order to meet the requirements of grouting water prevention and control strength, setting time, etc., the amount of industrial waste residue added is small, which cannot effectively reduce the grouting cost, and it is difficult to further improve the comprehensive performance of grouting materials.
[0009] Compared with the prior art, the industrial solid waste-based water-prevention grouting material provided by the present invention adds active gypsum, nano calcium carbonate and modified lime, and the three act synergistically to generate a network crystal mainly composed of calcium sulfonate, thereby ensuring the early and mid-term strength and interface bonding strength of the grouting material. At the same time, the three components have high reactivity and can promote the rapid progress of the hydration reaction, thereby effectively shortening the setting time; by adding a specific polymer emulsion, the compatibility between the components is enhanced, and the network adhesive film formed by the polymer emulsion after the slurry hardens is combined and entangled with the cement hydration product, which fills and seals the gaps inside the stone body, effectively preventing the generation of cracks in the stone body and preventing the penetration of water, and the generated network adhesive film has good softness and hydrophobicity, which can effectively improve the impermeability and flexural strength of the grouting material; through the synergistic effect of the above components, the addition amount of blast furnace slag and coal gangue is significantly increased, thereby effectively reducing the use of cement, achieving the purpose of increasing the amount of industrial solid waste added and reducing the grouting cost, realizing the comprehensive utilization of industrial solid waste, being more green and environmentally friendly, and having high practical value and promotion value.
[0010] Preferably, the specific surface area of the aluminophosphate cement clinker is ≥420m 2 / kg.
[0011] The aluminum phosphate cement clinker described in the present invention is a hydraulic cementitious material obtained by crushing and grinding limestone, bauxite and apatite as main raw materials into raw materials, and then calcining the raw materials at 1450° C. in a rotary kiln.
[0012] Preferably, the granulated blast furnace slag is S95 grade slag powder with a specific surface area of ≥420m 2 / kg.
[0013] The preferred granulated blast furnace slag has a higher activity, which can increase the hydration reaction rate of the slag, effectively shorten the early setting time, and produce the initial strength required for grouting.
[0014] Preferably, the coal gangue is red gangue, and the content of gangue with a particle size of ≤80µm in the coal gangue is not less than 85%.
[0015] During the stacking process, the gangue contains coal-containing substances, which will oxidize and spontaneously combust when exposed to air. The gangue after spontaneous combustion is fluffy and porous, commonly known as red gangue. Red gangue has certain volcanic ash properties and hydraulic properties. In the combined action of modified lime and activated gypsum, CSH gel and calcium aluminate can be quickly generated, which is beneficial to improve the early strength of the grouting material.
[0016] Preferably, the particle size of the nano calcium carbonate is 10nm-100nm.
[0017] The preferred nano calcium carbonate has high activity and mainly plays the role of crystal nucleus and filling in the grouting material. Adding nano calcium carbonate to the grouting material can increase the CSH gel content at the interface of different mineral materials in the grouting material, make the CSH tend to be non-directionally arranged, and the interface position transitions from a horizontal structure to a three-dimensional spatial structure, which is beneficial to increase the bonding strength at the interface and improve the durability and flexural strength of the grouting material; at the same time, nano calcium carbonate, as a crystal nucleus, can refine the crystal form of the hydration product of the grouting material, improve the submicrostructure of the grouting material, and promote the hydration reaction rate, thereby improving the early strength of the grouting material and shortening the setting time.
[0018] Preferably, the method for preparing the activated gypsum comprises the following steps: heating dihydrate gypsum to 750° C.-800° C. and keeping the temperature for 20 min-40 min to obtain the activated gypsum.
[0019] Calcination of gypsum at the above temperature can produce cavities inside the gypsum and distort the lattice of the gypsum, thereby significantly improving the activity of the gypsum and increasing the rate of hydration reaction. In addition, gypsum, together with modified lime and coal gangue, can generate network crystals mainly composed of calcium sulfonate, ensuring the early and mid-term strength and interface bonding strength of the grouting material.
[0020] Preferably, the polymer emulsion is a tetrahydrofurfuryl acrylate polymer modified polyacrylate emulsion and a styrene-acrylic acid copolymer in a mass ratio of 2-4:1.
[0021] The preparation method of the tetrahydrofurfuryl acrylate polymer modified polyacrylate emulsion is referred to CN109608586A.
[0022] The preferred polymer emulsion of the present invention can form an interwoven mesh membrane adhesive structure after hardening in the slurry, which separates the pores and plays a water-blocking role. The mesh membrane adhesive structure can also enhance the bonding strength of the components in the slurry, as well as the bonding strength between the slurry and the rock matrix. At the same time, the mesh adhesive film has good flexibility, which can effectively improve the compressive and flexural strength of the stone body and significantly improve the overall performance of the slurry.
[0023] Preferably, the preparation method of the modified lime comprises the following steps: calcining calcium acetate at 900° C.-950° C. for 1 h-2 h, and grinding to obtain modified lime with a fineness of ≥200 mesh.
[0024] The preferred preparation method of the modified lime can increase the specific surface area of the lime, form a polycrystalline structure of the lime, and improve the activity of the lime, so that the grouting material exhibits excellent performance in terms of setting time, stability, strength, etc. If the calcination temperature or the holding time is not within the above range, inactive CaO will be formed, reducing the activity of the modified lime.
[0025] Preferably, the composite admixture includes a water reducing agent and a nano material dispersant.
[0026] Preferably, the mass ratio of the water reducing agent to the nanomaterial dispersant is 1:1-2.
[0027] Preferably, the water reducing agent is naphthalenesulfonate formaldehyde polymer.
[0028] The preferred water reducing agent of the present invention can inhibit the volume shrinkage of the grouting material after solidification, reduce cracks caused by shrinkage, and enhance the impermeability, compressive strength and flexural strength of the grouting material.
[0029] Preferably, the nanomaterial dispersant is sodium dodecylbenzene sulfonate.
[0030] Adding nanomaterials to grouting materials will increase the viscosity of the slurry and increase the transportation resistance. At the same time, nanomaterials have small particle sizes and are easy to agglomerate in the slurry. In order to give full play to the role of nanomaterials and improve the workability of the slurry, the present invention adds naphthalenesulfonate formaldehyde polymer as a water reducer and sodium dodecylbenzenesulfonate as a dispersant, and controls the ratio of the two to ensure that the functions of the nanomaterials are fully exerted.
[0031] The present invention also provides a method for preparing an industrial solid waste-based water-based grouting material, comprising the following steps:
[0032] The components are weighed according to the designed proportions, and the weighed components are evenly mixed to obtain the industrial solid waste-based water-prevention grouting material.
[0033] The preparation method of the composite admixture provided by the present invention has simple material processing and production process, and the prepared grouting material has the advantages of high early strength, fast setting speed, low cost and good durability, and has high practical value and promotion value.
[0034] The present invention also provides a method for using the above-mentioned industrial solid waste-based water-prevention grouting material, which comprises mixing the industrial solid waste-based water-prevention grouting material with water evenly to obtain a slurry; using a grouting pump to transport the slurry to an area where the underground aquifer needs to be treated, reinforcing the bottom plate waterproof layer, performing grouting transformation on the aquifer, and sealing the water guide channel.
[0035] Exemplarily, the mass ratio of the industrial solid waste-based water-prevention grouting material to water is 1:1.
[0036] The industrial solid waste-based water-prevention grouting material provided by the present invention effectively improves the stability, early strength, setting speed and impermeability of the stone body by adding specific amounts of active gypsum, nano-calcium carbonate and modified lime, and adding a specific polymer emulsion, and greatly reduces the amount of cement added, effectively reduces the grouting cost, and also realizes the comprehensive utilization of industrial solid waste, has high economic and environmental benefits, and has extremely high value for promotion and application. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0038] The preparation methods of the activated gypsum and modified lime in the following examples are as follows:
[0039] Preparation method of activated gypsum: heat dihydrate gypsum to 780°C and keep it warm for 30 minutes to obtain activated gypsum.
[0040] The preparation method of the modified lime comprises the following steps: calcining calcium acetate at 1000° C. for 1.5 hours, and grinding the calcium acetate to obtain the modified lime with a fineness of ≥200 mesh.
[0041] The activated gypsum and modified lime prepared within the process parameter range defined by the present invention can achieve substantially equivalent technical effects.
[0042] The preparation method of tetrahydrofurfuryl acrylate polymer modified polyacrylate emulsion refers to CN109608586A.
[0043] Example 1
[0044] The embodiment of the present invention provides an industrial solid waste-based water grouting material for prevention and control, wherein the raw materials include the following components by weight:
[0045] 7 parts of phosphate aluminate cement clinker, 52 parts of granulated blast furnace slag, 20 parts of coal gangue, 5 parts of activated gypsum, 3 parts of nano calcium carbonate, 6 parts of polymer emulsion, 6 parts of modified lime and 0.3 parts of composite admixture;
[0046] The polymer emulsion is a tetrahydrofurfuryl acrylate polymer modified polyacrylate emulsion and a styrene-acrylic acid copolymer in a mass ratio of 3:1; the composite admixture is a naphthalenesulfonate formaldehyde polymer water reducer and a sodium dodecylbenzenesulfonate dispersant in a mass ratio of 1:1.5.
[0047] Among them, the specific surface area of phosphate aluminate cement clinker is 420m 2 / kg; Granulated blast furnace slag is S95 grade ore powder in accordance with GB / T18046-2017, with a specific surface area of 420m 2 / kg; the coal gangue is red gangue with a fineness of 80µm and a residual residue of 12% on a water sieve; the particle size of nano calcium carbonate is 50nm.
[0048] The preparation method of the above industrial solid waste-based water-based grouting material comprises the following steps:
[0049] The components are weighed according to the designed proportions, and the weighed components are evenly mixed to obtain the industrial solid waste-based water-prevention grouting material.
[0050] Example 2
[0051] The embodiment of the present invention provides an industrial solid waste-based water grouting material for prevention and control, wherein the raw materials include the following components by weight:
[0052] 10 parts of phosphate aluminate cement clinker, 41 parts of granulated blast furnace slag, 28 parts of coal gangue, 10 parts of activated gypsum, 4 parts of nano calcium carbonate, 3 parts of polymer emulsion, 4 parts of modified lime and 0.4 parts of composite admixture;
[0053] The polymer emulsion is a tetrahydrofurfuryl acrylate polymer modified polyacrylate emulsion and a styrene-acrylic acid copolymer in a mass ratio of 2:1; the composite admixture is a naphthalenesulfonate formaldehyde polymer water reducer and a sodium dodecylbenzenesulfonate dispersant in a mass ratio of 1:2.
[0054] Among them, the specific surface area of phosphate aluminate cement clinker is 420m 2 / kg; Granulated blast furnace slag is S95 grade ore powder in accordance with GB / T18046-2017, with a specific surface area of 420m 2 / kg; the coal gangue is red gangue with a fineness of 80µm and a residual residue of 13% on a water sieve; the particle size of nano calcium carbonate is 10nm.
[0055] The preparation method of the above industrial solid waste-based water-based grouting material comprises the following steps:
[0056] The components are weighed according to the designed proportions, and the weighed components are evenly mixed to obtain the industrial solid waste-based water-prevention grouting material.
[0057] Example 3
[0058] The embodiment of the present invention provides an industrial solid waste-based water grouting material for prevention and control, wherein the raw materials include the following components by weight:
[0059] 5 parts of phosphate aluminate cement clinker, 58 parts of granulated blast furnace slag, 20 parts of coal gangue, 3 parts of activated gypsum, 5 parts of nano calcium carbonate, 8 parts of polymer emulsion, 8 parts of modified lime and 0.5 parts of composite admixture;
[0060] The polymer emulsion is a tetrahydrofurfuryl acrylate polymer modified polyacrylate emulsion and a styrene-acrylic acid copolymer in a mass ratio of 4:1; the composite admixture is a naphthalenesulfonate formaldehyde polymer water reducer and a sodium dodecylbenzenesulfonate dispersant in a mass ratio of 1:1.
[0061] Among them, the specific surface area of phosphate aluminate cement clinker is 420m 2 / kg; Granulated blast furnace slag is S95 grade ore powder in accordance with GB / T18046-2017, with a specific surface area of 420m 2 / kg; the coal gangue is red gangue with a fineness of 80µm and a residual on the sieve of 14%; the particle size of nano calcium carbonate is 100nm.
[0062] The preparation method of the above industrial solid waste-based water-based grouting material comprises the following steps:
[0063] The components are weighed according to the designed proportions, and the weighed components are evenly mixed to obtain the industrial solid waste-based water-prevention grouting material.
[0064] Example 4
[0065] This embodiment provides an industrial solid waste-based water grouting material for prevention and control, and its composition and preparation method are exactly the same as those in Example 1, except that the preparation method of the modified lime is different:
[0066] Calcium acetate was calcined at 1200°C for 1.5 h and ground to obtain modified lime.
[0067] Comparative Example 1
[0068] This comparative example provides an industrial solid waste-based water-prevention grouting material, whose component composition and preparation method are exactly the same as those in Example 1, except that the tetrahydrofurfuryl acrylate polymer-modified polyacrylate emulsion in the polymer emulsion is replaced by an equal amount of polyacrylate emulsion (Hongya Jianye Building Materials).
[0069] Comparative Example 2
[0070] This comparative example provides an industrial solid waste-based water-prevention grouting material, the composition and preparation method of which are exactly the same as those of Example 1, except that the active gypsum is replaced by an equal amount of anhydrite.
[0071] Comparative Example 3
[0072] This comparative example provides an industrial solid waste-based water-prevention grouting material, the component composition and preparation method of which are exactly the same as those of Example 1, except that the phosphate aluminate cement clinker is replaced by an equal amount of silicate cement.
[0073] Performance Testing
[0074] In order to demonstrate the effects of the grouting materials prepared in the embodiments and comparative examples of the present invention, the grouting materials in embodiments 1-4 and comparative examples 1-3 were subjected to performance tests, and the specific test conditions were as follows:
[0075] Coagulation time determination:
[0076] The grouting materials prepared in Examples 1-4 and Comparative Examples 1-3 and water were poured into a cement slurry mixer at a mass ratio of 1:1, stirred slowly for 120 seconds, poured into a cup-shaped container, and stopped pouring after the slurry liquid level reached a fixed position. The cup-shaped container was placed in a curing box for curing. The curing conditions were in accordance with the provisions of GB / T 17671-1999, Part 8. The specimen was cured in the curing box until 10 hours after adding water for the first measurement. The specimen was placed under the initial setting needle of the Vicat instrument. Because there was a water seepage layer on the upper part of the slurry in the specimen, the initial setting needle was required to pass through the water seepage layer and approach the slurry surface. The pointer height was adjusted so that the Vicat instrument reading was 25 mm. The screw was tightened for 1-2 seconds, and suddenly released. The test needle vertically and freely sank into the grouting slurry. The reading when the test needle stopped sinking was observed. The specimen whose test needle sank into the slurry and sank 6 mm ± 1 mm was in the initial setting state, and the specimen was recorded.
[0077] Strength detection:
[0078] Preparation of mortar: The test blocks of grouting materials shall be prepared in accordance with the provisions of 6 of GB / T 17617-1999.
[0079] Preparation of test pieces: The test pieces of grouting materials shall be prepared in accordance with the provisions of 7 of GB / T 17617-1999.
[0080] Specimen curing: in accordance with the provisions of GB / T 17671-1999, Part 8.
[0081] Strength test: according to 9.2 and 9.3 of GB / T 17671-1999.
[0082] The results are shown in Tables 1 to 3.
[0083] Table 1 Compressive strength test results
[0084]
[0085] Table 2 Flexural strength test results
[0086]
[0087] Table 3 Coagulation time test results
[0088] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Coagulation time (h) 14.1 13.5 14.3 15.5 16.8 17.5 18.5
[0089] To sum up, the industrial solid waste-based water-prevention grouting material provided by the present invention has a large amount of industrial solid waste added, and the various components of the material cooperate with each other to regulate the early hydration microstructure of the grouting material and reduce its internal defects. It can significantly improve the impermeability, strength and toughness of the grouting material, shorten the setting time of the grouting material, and extend the service life of the grouting material, and has broad application prospects.
[0090] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An industrial solid waste-based water-prevention grouting material, characterized in that: The invention comprises the following raw material components in parts by weight: 5-10 parts of phosphate aluminate cement clinker, 40-60 parts of granulated blast furnace slag, 20-30 parts of coal gangue, 3-10 parts of activated gypsum, 2-5 parts of nano calcium carbonate, 3-10 parts of polymer emulsion, 4-10 parts of modified lime and 0.1-0.5 parts of composite admixture; Wherein, the polymer emulsion comprises tetrahydrofurfuryl acrylate polymer modified polyacrylate emulsion and styrene-acrylic acid copolymer; The preparation method of the active gypsum comprises the following steps: heating dihydrate gypsum to 750° C.-800° C. and keeping the temperature for 20 min-40 min to obtain the active gypsum.
2. The industrial solid waste-based water grouting material for prevention and control of water according to claim 1, characterized in that: The specific surface area of the aluminophosphate cement clinker is ≥420m 2 / kg; and / or The granulated blast furnace slag is S95 grade slag powder with a specific surface area of ≥420m 2 / kg; and / or The coal gangue is red gangue, and the content of gangue with a particle size of ≤80µm in the coal gangue is not less than 85%; and / or The particle size of the nano calcium carbonate is 10nm-100nm.
3. The industrial solid waste-based water grouting material for prevention and control of water according to claim 1, characterized in that: The polymer emulsion is a tetrahydrofurfuryl acrylate polymer modified polyacrylate emulsion and a styrene-acrylic acid copolymer in a mass ratio of 2-4:
1.
4. The industrial solid waste-based water grouting material for prevention and control as claimed in claim 1, characterized in that: The preparation method of the modified lime comprises the following steps: calcining calcium acetate at 900° C.-950° C. for 1 h-2 h, and grinding to obtain modified lime with a fineness of ≥200 mesh.
5. The industrial solid waste-based water grouting material for prevention and control as claimed in claim 1, characterized in that: The composite admixture comprises a water reducing agent and a nano material dispersant.
6. The industrial solid waste-based water grouting material for prevention and control as claimed in claim 5, characterized in that: The water reducing agent is a naphthalenesulfonate formaldehyde polymer; and / or The nano material dispersant is sodium dodecylbenzene sulfonate.
7. The industrial solid waste-based water grouting material for prevention and control as claimed in claim 5 or 6, characterized in that: The mass ratio of the water reducing agent to the nano material dispersant is 1:1-2.
8. The method for preparing the industrial solid waste-based water grouting material for prevention and control according to any one of claims 1 to 7, characterized in that: The steps include: The components are weighed according to the designed proportions, and the weighed components are evenly mixed to obtain the industrial solid waste-based water-prevention grouting material.
9. The method for using the industrial solid waste-based water grouting material for prevention and control according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: uniformly mixing the industrial solid waste-based water-control grouting material with water to obtain slurry; and using a grouting pump to transport the slurry to an area where the underground aquifer needs to be treated for coagulation and reinforcement.
Citation Information
Cited By
Sandy soil solidification method based on synergistic effect of MICP and organic polymer emulsion
CN121275450A