A polymer insulating material for coating overhead wires and a preparation method thereof
By preparing polymer insulating materials containing vinyl hydroxy silicone resin and other components, the problems of overhead bare wires are easily corroded and leakage, and the insulation effect with high breakdown voltage and long life is achieved. It is suitable for 35kV overhead wires.
Patent Information
- Application Number
- CN202310432300.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-20
AI Technical Summary
The prior art lacks high voltage and corrosion resistant insulating materials for coating overhead bare wires, resulting in the occurrence of corrosive and leakage accidents in the wires.
A polymer insulating material is used, containing vinyl hydroxy silicone resin, nano-hydrophobic reinforced white carbon black, hydrophobic polytetrafluoroethylene powder, hydrophobic silica, platinum catalytic flame retardant, coupling agent, deketoxime type crossing Coupling agent and organotin catalyst are used to prepare a single-component high viscosity and room temperature cured liquid insulating material through specific stirring and grinding treatment methods.
This material can tightly wrap overhead bare wires to prevent leakage accidents. The AC breakdown voltage can reach 50kV/4mm, the service life is more than 15 years, and it cures quickly at room temperature, making it suitable for power-on operation.
Smart Images

Figure CN116515390B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of insulating materials, and in particular to a polymer insulating material for coating overhead conductors and a preparation method thereof. Background Art
[0002] The biggest feature of the early overhead bare wires is that they are conducive to heat dissipation during use and are cheap, so they are generally used for outdoor distribution line installation. In order to increase the tensile strength of the wire, it is often necessary to twist the aluminum wire and the steel wire outside the steel core wire, which is called "steel core aluminum stranded wire". Since the bare wire has no insulating sheath, the wire is directly exposed to the atmospheric environment and is easily corroded. In addition, the use of it in densely populated areas, near tree areas, and cross-domains of lines (rivers, ponds, viaducts, etc.) is prone to cause accidents. Therefore, in the process of power grid transformation, overhead bare wires have been gradually replaced by overhead insulated wires. Overhead insulated wires are transmission wires with an insulating layer wrapped around their outer layer. Because of the protection of the insulating layer, the contact with the air is reduced, the possibility of oxidation and corrosion of the wire core is greatly reduced, and the service life of the line is extended. Similarly, the impact of external adverse factors such as dust and floating objects on the wire is also reduced. More importantly, the insulating layer greatly improves the external insulation performance of the line and reduces the occurrence of phase-to-phase short circuits and human electric shock accidents.
[0003] Therefore, the high voltage resistant and corrosion resistant insulating material used for coating on overhead bare conductors needs to be further developed and improved. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a polymer insulating material for coating overhead wires and a preparation method thereof, aiming to solve the problem that the prior art lacks high-voltage and corrosion-resistant insulating materials for coating overhead bare wires.
[0005] The technical solution of the present invention is as follows:
[0006] A polymer insulating material for coating an overhead conductor comprises, by weight: 50-80 parts of vinyl hydroxy silicone resin, 10-30 parts of nano hydrophobic reinforcing white carbon black, 10-30 parts of hydrophobic polytetrafluoroethylene powder, 5-20 parts of hydrophobic silicon dioxide, 0.5-2 parts of platinum catalytic flame retardant, 2-10 parts of coupling agent, 5-12 parts of deketoxime type crosslinking agent, 0.2-1 parts of pigment and 0.05-1 parts of organic tin catalyst.
[0007] The polymer insulating material for coating overhead wires, wherein the polymerization degree of the vinyl hydroxy silicone resin is 500-80000, the vinyl content is 0.1-2.0%, and the hydroxyl content is 0.1-1.0%.
[0008] The polymer insulating material for coating overhead wires, wherein the specific surface area of the nano hydrophobic reinforcing white carbon black is 100-600m 2 / g.
[0009] The polymer insulating material for coating overhead wires, wherein the fineness of the hydrophobic polytetrafluoroethylene powder is 3000-15000 meshes, and the fineness of the hydrophobic silicon dioxide is 5000-15000 meshes.
[0010] The polymer insulating material for coating overhead wires, wherein the coupling agent is a mixture of vinyltrimethoxysilane and methyltrimethoxysilane.
[0011] The polymer insulating material for coating overhead wires, wherein the deketoxime type cross-linking agent is a mixture of methyltributylacetoximine silane and vinyltributylacetoximine silane.
[0012] The polymer insulating material for coating overhead wires, wherein the organic tin catalyst is one or both of organic tin carboxylate and organic tin chelate.
[0013] A method for preparing a polymer insulating material for coating an overhead conductor, comprising the steps of:
[0014] Add vinyl hydroxy silicone resin, nano hydrophobic reinforcing white carbon black, hydrophobic polytetrafluoroethylene powder, hydrophobic silica and pigment into a disperser by weight, stir and disperse, and then perform vacuum treatment, while heating until the material temperature reaches a first predetermined temperature, and after maintaining the first predetermined time, pass cooling water to cool the material temperature to a second predetermined temperature to obtain a mixture;
[0015] The mixture is transferred to a three-roll grinder for grinding, and then transferred to a disperser. A platinum catalytic flame retardant, a coupling agent, and a deketoxime type cross-linking agent are added. The disperser is evacuated and cooled with water. The disperser is started, and the temperature is controlled below a third predetermined temperature. After the temperature is maintained for a second predetermined time, an organic tin catalyst is added. The mixture is evacuated again and the disperser is started for stirring and dispersing for a third predetermined time to obtain the polymer insulating material.
[0016] The preparation method of the polymer insulating material for coating overhead wires, wherein the first predetermined temperature is 100-150°C, the first predetermined time is 1-3h; the second predetermined temperature is 50-70°C; the third predetermined temperature is 50-70°C, the second predetermined time is 0.5-1.5h; the third predetermined time is 20-40min.
[0017] The method for preparing the polymer insulating material for coating overhead wires, wherein the rotation speed of the disperser is 1800-2500 r / min.
[0018] Beneficial effect: The present invention develops a polymer insulation material for 35kV overhead bare conductors. The material is a single-component high-viscosity liquid insulation material that solidifies at room temperature. Its solid content is 100% and its density is 1.3-1.4g / cm 3 , by using a special coating robot, the insulating material is coated on a 35kV overhead bare conductor, which can insulate the surface of the bare conductor and tightly wrap the overhead bare conductor to prevent leakage accidents. The high-density insulating material provided by the present invention has been tested many times, and its AC breakdown voltage can reach 50kV / 4mm. Due to the silicone system, its silicone resin content reaches more than 50%, and its service life reaches more than 15 years. The polymer insulating material provided by the present invention is cured at room temperature, the surface curing time is 30min, and the complete curing time is 12h. It can be coated on the overhead bare conductor and powered on without affecting its load-bearing capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The present invention is a flow chart of a method for preparing a polymer insulating material for coating overhead conductors. DETAILED DESCRIPTION
[0020] The present invention provides a polymer insulating material for coating an overhead conductor and a preparation method thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0021] The invention provides a polymer insulating material for coating an overhead wire. The polymer insulating material comprises, by weight, 50-80 parts of vinyl hydroxy silicone resin, 10-30 parts of nano hydrophobic reinforcing white carbon black, 10-30 parts of hydrophobic polytetrafluoroethylene powder, 5-20 parts of hydrophobic silicon dioxide, 0.5-2 parts of a platinum catalytic flame retardant, 2-10 parts of a coupling agent, 5-12 parts of a deketoxime type crosslinking agent, 0.2-1 parts of a pigment and 0.05-1 parts of an organic tin catalyst.
[0022] In the present invention, the nano hydrophobic silica can be effectively combined with the vinyl hydroxy silicone resin through the Si-0 bond, and the deketoxime crosslinking agent can be pre-polymerized with the vinyl hydroxy silicone resin and the nano hydrophobic silica, effectively improving the thixotropy of the material, producing a fixed shape, and effectively preventing the material from flowing. When used, it does not deform at a thickness of 10 mm, ensuring uniformity; in the present invention, the dielectric constant of the hydrophobic polytetrafluoroethylene powder is very low, and adding 10-30 parts of the hydrophobic polytetrafluoroethylene powder can effectively improve the insulation strength of the insulating material; in the present invention, the vinyl hydroxy silicone resin is used as the main component to improve the insulation strength and service life of the insulating material.
[0023] In some embodiments, the degree of polymerization of the vinyl hydroxy silicone resin is 500-80000, its vinyl content is 0.1-2.0%, and the hydroxyl content is 0.1-1.0%. In the present embodiment, if the degree of polymerization of the vinyl hydroxy silicone resin is too low (less than 500), the vinyl hydroxy silicone resin is easy to become hard and brittle after cross-linking, and if the degree of polymerization of the vinyl hydroxy silicone resin is too high (greater than 80000), the vinyl hydroxy silicone resin becomes overly soft after cross-linking and fails to reach the required strength. In the present embodiment, the vinyl content in the vinyl hydroxy silicone resin is relatively high. Since the vinyl is a non-polar bond, a high vinyl content can improve the insulation strength. In the present embodiment, the hydroxyl group in the vinyl hydroxy silicone resin is the main functional group used for condensation reaction. Too low results in low reaction functionality and low strength, and too high results in incomplete hydroxyl reaction. Since the hydroxyl group is a polar bond, too many hydroxyl groups are prone to affect the insulation performance.
[0024] In some embodiments, the specific surface area of the nano hydrophobic reinforced silica is 100-600 m 2 / g. White carbon black is a general term for white powdered X-ray amorphous silicic acid and silicate products, mainly referring to precipitated silica, fumed silica and ultrafine silica gel, and also including powdered synthetic aluminum silicate and calcium silicate. White carbon black is a porous substance, and its composition can be expressed by SiO2·nH2O, where nH2O exists in the form of surface hydroxyl groups. White carbon black itself is hydrophilic, and hydrophobic white carbon black is modified by hydrophobic groups. Hydrophobic white carbon black is prepared by chemical reaction of hydrophilic fumed white carbon black with active silane (such as chlorosilane or hexamethyldisilazane). It is hydrophobic (water-repellent) and cannot be dispersed in water. The nano hydrophobic reinforcing white carbon black can be used to reinforce silicone elastomers; it has good hydrophobicity and can improve corrosion resistance; and it can also improve the dielectric properties of cable composites or improve scratch resistance. In this embodiment, the nano hydrophobic reinforcing white carbon black mainly plays a thixotropic role, which can improve the shaping property of the material, and also plays a reinforcing and hydrophobic role, effectively preventing water vapor from entering the material and improving the insulation performance under humid conditions. In this embodiment, the larger the specific surface area of the nano hydrophobic reinforcing white carbon black is theoretically, the better the reinforcing performance is. Considering all factors, a specific surface area of 150-200m2 / g is cost-effective.
[0025] In some embodiments, the effective concentration of the platinum catalytic flame retardant is 1000-20000 ppm / g. In this embodiment, the main component of the platinum catalytic flame retardant is platinum ions, such as platinum ions extracted from chloroplatinic acid, which mainly play a flame retardant role.
[0026] In some embodiments, the fineness of the hydrophobic polytetrafluoroethylene powder is 3000-15000 mesh, and the fineness of the hydrophobic silicon dioxide is 5000-15000 mesh. In this embodiment, the hydrophobic silicon dioxide is used to strengthen the hydrophobicity and increase the hardness; the hydrophobic polytetrafluoroethylene powder is used to improve the insulation performance.
[0027] In some embodiments, the coupling agent is a mixture of vinyl trimethoxy silane and methyl trimethoxy silane. In this embodiment, the coupling agent is mainly used to improve the adhesion between the material and the aluminum wire. When the mixture of vinyl trimethoxy silane and methyl trimethoxy silane is used as the coupling agent, the adhesion of the obtained polymer insulating material can be as high as level 1 or above.
[0028] In some embodiments, the deketoxime crosslinking agent is a mixture of methyltributylacetoximosilane and vinyltributylacetoximosilane. In this embodiment, the methyltributylacetoximosilane reacts faster, while the vinyltributylacetoximosilane reacts slower. The reaction rate can be adjusted by mixing the two.
[0029] In some embodiments, the organotin catalyst is one or both of an organic tin carboxylate and an organic tin chelate. In this embodiment, the organotin catalyst is mainly used at a temperature below 10° C. Addition can increase the reaction rate.
[0030] In some embodiments, a method for preparing a polymer insulating material for coating an overhead conductor is also provided. Figure 1 As shown, it includes the steps of:
[0031] S10, adding vinyl hydroxy silicone resin, nano hydrophobic reinforcing white carbon black, hydrophobic polytetrafluoroethylene powder, hydrophobic silica and pigment into a disperser by weight, stirring and dispersing, and then vacuuming, while heating until the material temperature reaches a first predetermined temperature, and after maintaining the first predetermined time, cooling water is passed to cool the material temperature to a second predetermined temperature to obtain a mixture;
[0032] S20, transferring the mixture to a three-roll grinder for grinding, then transferring the mixture to a disperser, adding a platinum catalytic flame retardant, a coupling agent, and a deketoxime type cross-linking agent, evacuating the disperser, passing cooling water, starting the disperser, controlling the temperature below a third predetermined temperature, maintaining the temperature for a second predetermined time, adding an organic tin catalyst, evacuating the mixture again, and starting the disperser for stirring and dispersing for a third predetermined time to obtain the polymer insulating material.
[0033] Specifically, in this embodiment, vinyl hydroxy silicone resin, nano hydrophobic reinforcing white carbon black, hydrophobic polytetrafluoroethylene powder, hydrophobic silica and black pigment are first added to a disperser, the disperser is started, the speed is 1800-2500r / min, and then vacuumed to -0.1mpa, and the temperature is raised at the same time until the material temperature reaches 100-150°C, the holding time is 1-3h, and then the cooling water is passed to cool the material to a temperature of 50-70°C to obtain the mixture; then, the mixture is transferred to a three-roll grinder, the cooling water is turned on, the gap of the grinder is adjusted to 30um, and the mixture is ground twice until the mixture is The fineness of the mixed material reaches 30um, and then the mixed material is transferred to a disperser, and platinum catalytic flame retardant, coupling agent, and deketoxime type cross-linking agent are added. The mixture is evacuated to -0.1mpa, and cooling water is passed at the same time. The disperser is started with a speed of 1800-2500r / min, and the temperature is controlled below 50-70℃ for 0.5-1.5h; then an organic tin catalyst is added, the mixture is evacuated to -0.1mpa, and the disperser is started with a speed of 1800-2500r / min for 20-40min. The discharge is sealed and the obtained polymer insulating material is packaged with a special packaging machine.
[0034] The polymer insulating material prepared by the method of this embodiment is a single-component high-viscosity liquid insulating material that solidifies at room temperature, and its solid content is 100% and its density is 1.3-1.4 g / cm3 , by using a special coating robot, the polymer insulation material is coated on a 35kV overhead bare conductor, which can insulate the surface of the bare conductor and tightly wrap the overhead bare conductor to prevent leakage accidents. The high-density insulation material provided by the present invention has been tested many times, and its AC breakdown voltage can reach 50kV / 4mm. Due to the silicone system, its silicone resin content reaches more than 50%, and its service life reaches more than 15 years. The polymer insulation material provided by the present invention is cured at room temperature, the surface curing time is 30min, and the complete curing time is 12h. It can be coated on the overhead bare conductor and powered on without affecting its load-bearing capacity.
[0035] The present invention will be further explained below by means of specific embodiments:
[0036] Example 1
[0037] A polymer insulating material for coating an overhead conductor comprises, by weight: 65 parts of vinyl hydroxy silicone resin, 20 parts of nano hydrophobic reinforcing white carbon black, 20 parts of hydrophobic polytetrafluoroethylene powder, 10 parts of hydrophobic silica, 1 part of platinum catalytic flame retardant, 6 parts of coupling agent, 8 parts of deketoxime type cross-linking agent, 0.5 parts of pigment and 0.5 parts of organic tin catalyst.
[0038] The preparation of the polymer insulating material in this embodiment includes the following steps:
[0039] 1. First, vinyl hydroxy silicone resin, nano hydrophobic reinforcing white carbon black, hydrophobic polytetrafluoroethylene powder, hydrophobic silica and black pigment are added to a disperser, and the disperser is started at a speed of 2000r / min, and then vacuumed to -0.1mpa, and the temperature is increased at the same time until the material temperature reaches 120°C, and the temperature is maintained for 2h, and then cooling water is passed to cool the material temperature to 60°C to obtain the mixed material;
[0040] 2. Transfer the mixture to a three-roll grinder, turn on the cooling water, adjust the gap of the grinder to 30um, grind twice until the fineness of the mixture reaches 30um, then transfer the mixture to a disperser, add a platinum catalytic flame retardant, a coupling agent, and a deketoxime type cross-linking agent, evacuate to -0.1 MPa, pass cooling water at the same time, start the disperser, the speed is 2000r / min, the temperature is controlled below 60°C, and maintained for 1h; then add an organic tin catalyst, evacuate to -0.1 MPa, start the disperser, the speed is 2000r / min, maintain for 30min, seal the discharge, and use a special packaging machine to package the obtained polymer insulating material.
[0041] Example 2
[0042] A polymer insulating material for coating an overhead conductor comprises, by weight: 50 parts of vinyl hydroxy silicone resin, 10 parts of nano hydrophobic reinforcing white carbon black, 10 parts of hydrophobic polytetrafluoroethylene powder, 5 parts of hydrophobic silica, 0.5 parts of platinum catalytic flame retardant, 2 parts of coupling agent, 5 parts of deketoxime type crosslinking agent, 0.2 parts of pigment and 0.05 parts of organic tin catalyst.
[0043] The preparation of the polymer insulating material in this embodiment includes the following steps:
[0044] 1. First, vinyl hydroxy silicone resin, nano hydrophobic reinforcing white carbon black, hydrophobic polytetrafluoroethylene powder, hydrophobic silica and black pigment are added to a disperser, and the disperser is started at a speed of 1800 r / min, and then vacuumed to -0.1 MPa, and the temperature is raised at the same time until the material temperature reaches 100° C., and the temperature is maintained for 1 hour, and then cooling water is passed to cool the material temperature to 50° C. to obtain the mixed material;
[0045] 2. Transfer the mixture to a three-roll grinder, turn on the cooling water, adjust the gap of the grinder to 30um, grind twice until the fineness of the mixture reaches 30um, then transfer the mixture to a disperser, add a platinum catalytic flame retardant, a coupling agent, and a deketoxime type cross-linking agent, evacuate to -0.1 MPa, pass cooling water at the same time, start the disperser, the speed is 1800 r / min, the temperature is controlled below 50°C, and maintained for 0.5h; then add an organic tin catalyst, evacuate to -0.1 MPa, start the disperser, the speed is 1800 r / min, maintain for 20min, seal the discharge, and use a special packaging machine to package the obtained polymer insulating material.
[0046] Example 3
[0047] A polymer insulating material for coating an overhead conductor comprises, by weight: 80 parts of vinyl hydroxy silicone resin, 30 parts of nano hydrophobic reinforcing white carbon black, 30 parts of hydrophobic polytetrafluoroethylene powder, 20 parts of hydrophobic silica, 2 parts of platinum catalytic flame retardant, 10 parts of coupling agent, 12 parts of deketoxime type cross-linking agent, 1 part of pigment and 1 part of organic tin catalyst.
[0048] The preparation of the polymer insulating material in this embodiment includes the following steps:
[0049] 1. First, vinyl hydroxy silicone resin, nano hydrophobic reinforcing white carbon black, hydrophobic polytetrafluoroethylene powder, hydrophobic silica and black pigment are added to a disperser, and the disperser is started at a speed of 2500r / min, and then vacuumed to -0.1mpa, and the temperature is raised at the same time until the material temperature reaches 150°C, and the temperature is maintained for 3h, and then cooling water is passed to cool the material temperature to 70°C to obtain the mixed material;
[0050] 2. Transfer the mixture to a three-roll grinder, turn on the cooling water, adjust the gap of the grinder to 30um, grind twice until the fineness of the mixture reaches 30um, then transfer the mixture to a disperser, add a platinum catalytic flame retardant, a coupling agent, and a deketoxime type cross-linking agent, evacuate to -0.1 MPa, pass cooling water at the same time, start the disperser, the speed is 2500r / min, the temperature is controlled below 70°C, and maintain for 1.5h; then add an organic tin catalyst, evacuate to -0.1 MPa, start the disperser, the speed is 2500r / min, maintain for 40min, seal the discharge, and use a special packaging machine to package the obtained polymer insulating material.
[0051] Test Case
[0052] The polymer insulation material prepared in Example 1 was coated on a 35kV overhead bare conductor to insulate the surface of the bare conductor and form an insulating layer, thereby obtaining an overhead insulated conductor. The obtained overhead insulated conductor was sent to Shanghai Electric Equipment Testing Institute Co., Ltd. for third-party performance testing, and the test results are shown in Table 1.
[0053] Table 1
[0054]
[0055]
[0056]
[0057]
[0058] The above test data is obtained according to the following standards:
[0059] 1. GB / T 2423.2-2008 "Environmental testing for electric and electronic products Part 2: Test methods Test B: High temperature";
[0060] 2. GB / T 1410-2006 Test method for volume resistivity and surface resistivity of solid insulating materials;
[0061] 3. GB / T 1409-2006 "Recommended method for measuring the permittivity and dielectric loss factor of electrical insulating materials at power frequency, audio frequency and high frequency (including meter wave wavelength)";
[0062] 4. GB / T 3048.4-2007 "Electrical performance test methods for wires and cables Part 4: Conductor DC resistance test";
[0063] 5. GB / T 16422.2-2014 "Plastics Laboratory Light Source Exposure Test Methods Part 2: Xenon Arc Lamp";
[0064] 6. GB / T 18380.12-2008 "Combustion tests for electric and optical cables under flame conditions - Part 12: Vertical flame spread test for single insulated wires and cables - 1kW premixed flame test method";
[0065] 7. GB / T 1408.1-2016 "Electrical strength test methods for insulating materials Part 1: Tests at power frequency";
[0066] 8. GB / T 1033.1-2008 “Plastics - Determination of density of non-foamed plastics”.
[0067] It can be seen from the test results in Table 1 that the polymer insulating material prepared in Example 1 of the present invention is a single-component high-viscosity liquid insulating material that cures at room temperature, with a solid content of 100% and a density of 1.3 g / cm 3 By using a dedicated coating robot, this polymer insulation material is coated on a 35kV overhead bare conductor, and its surface resistivity is as high as 5.50×10 14 Ω, volume resistivity up to 1.64×10 12 Ω·m, the dielectric constant is 3.2085, which can insulate the surface of the bare wire and can tightly wrap the overhead bare wire to prevent the occurrence of leakage accidents. The high-density insulating material provided by the present invention has been tested many times, and its AC breakdown voltage can reach 50kV / 4mm. Due to the silicone system, its silicone resin content reaches more than 50%, and its service life reaches more than 15 years. The polymer insulating material provided by the present invention is cured at room temperature, the surface curing time is 30min, and the complete curing time is 12h. It can be coated on the overhead bare wire and powered on without affecting its load-bearing capacity. In the data in Table 1, the breakdown voltage in sequence number 6 refers to the breakdown voltage of the standard 2mm thickness film, and the cable breakdown voltage in sequence number 7 refers to the breakdown voltage of the 4mm thick coated cable.
[0068] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A polymer insulating material for coating overhead wires, characterized in that: The invention comprises, by weight, 50-80 parts of vinyl hydroxy silicone resin, 10-30 parts of nano hydrophobic reinforcing white carbon black, 10-30 parts of hydrophobic polytetrafluoroethylene powder, 5-20 parts of hydrophobic silica, 0.5-2 parts of platinum catalytic flame retardant, 2-10 parts of coupling agent, 5-12 parts of deketoxime crosslinking agent, 0.2-1 parts of pigment and 0.05-1 parts of organic tin catalyst; the polymerization degree of the vinyl hydroxy silicone resin is 500-80000, the vinyl content is 0.1-2.0%, and the hydroxyl content is 0.1-1.0%; the specific surface area of the nano hydrophobic reinforcing white carbon black is 100-600m 2 / g; the fineness of the hydrophobic polytetrafluoroethylene powder is 3000-15000 mesh, and the fineness of the hydrophobic silica is 5000-15000 mesh; the coupling agent is a mixture of vinyltrimethoxysilane and methyltrimethoxysilane; the deketoxime type cross-linking agent is a mixture of methyltributylanoxime silane and vinyltributylanoxime silane; the organic tin catalyst is one or two of organic carboxylic acid tin and organic tin chelate.
2. A method for preparing a polymer insulating material for coating an overhead conductor as claimed in claim 1, characterized in that: Includes steps: Add vinyl hydroxy silicone resin, nano hydrophobic reinforcing white carbon black, hydrophobic polytetrafluoroethylene powder, hydrophobic silica and pigment into a disperser by weight, stir and disperse, and then perform vacuum treatment, while heating until the material temperature reaches a first predetermined temperature, and after maintaining the first predetermined time, pass cooling water to cool the material temperature to a second predetermined temperature to obtain a mixture; The mixture is transferred to a three-roll grinder for grinding, and then transferred to a disperser. A platinum catalytic flame retardant, a coupling agent, and a deketoxime type cross-linking agent are added. The disperser is evacuated and cooled with water. The disperser is started, and the temperature is controlled below a third predetermined temperature. After the temperature is maintained for a second predetermined time, an organic tin catalyst is added. The mixture is evacuated again and the disperser is started for stirring and dispersing for a third predetermined time to obtain the polymer insulating material.
3. The method for preparing a polymer insulating material for coating overhead wires according to claim 2, characterized in that: The first predetermined temperature is 100-150°C, and the first predetermined time is 1-3h; the second predetermined temperature is 50-70°C; the third predetermined temperature is 50-70°C, and the second predetermined time is 0.5-1.5h; the third predetermined time is 20-40min.
4. The method for preparing a polymer insulating material for coating overhead wires according to claim 2, characterized in that: The rotating speed of the disperser is 1800-2500 r / min.