Silver-glazed Jianzhan with earthworm-walking-in-mud pattern and preparation method thereof

By rationally proportioning the glaze raw materials and firing process, the problem of lack of earthworm mud patterns and high cost in the existing silver-glazed pots has been solved, and a low-cost, stable-fired silver-glazed pot with high wear resistance has been achieved. properties and gloss, and the yield is high, reducing the waste of raw materials.

CN116535096BActive Publication Date: 2024-10-29SHAANXI UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310536386.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-10-29
Estimated Expiration
2043-05-12

AI Technical Summary

Technical Problem

In the existing technology, there are no reports on the firing and analysis of silver-glazed pots with earthworm mud patterns, and multi-layer glazing results in high production costs, poor yields, and waste of ceramic raw material resources.

Method used

By rationally proportioning the glaze raw materials, including feldspar, manganese oxide, cobalt oxide and high content of ferric oxide, using one-time glazing and wet ball milling process, combined with the firing process of oxidation and reduction atmosphere, silver luster and earthworm walking are formed. Mud pattern.

Benefits of technology

The low-cost and stable firing of silver-glazed wares with earthworm mud patterns has been achieved, which has improved the wear resistance, gloss and yield of the glaze, enriched the types of black-glazed porcelain, and reduced the waste of raw materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004226400970000011
    Figure HDA0004226400970000011
Patent Text Reader

Abstract

The invention provides a silver-glazed Jianzhan with earthworm mud patterns and a preparation method thereof, comprising the following steps: (1) preparing glaze raw materials into glaze; the glaze raw materials include: 50-70 parts of feldspar, 2-8 parts of kaolin, 15-25 parts of quartz, 10-16 parts of calcite, 0.5-2 parts of talc, 1-3 parts of tricalcium phosphate, 5-10 parts of boron frit, 0.1-0.6 parts of sodium tripolyphosphate, 0.5-1.5 parts of sodium carboxymethyl cellulose, 5-10 parts of ferric oxide, 1-2 parts of manganese dioxide, and 0.2-1 parts of cobalt oxide; (2) dipping a blank into the glaze once, the dipping time is 10-20s, and drying; (3) heating the dried blank to 900°C in an oxidizing atmosphere, heating to 1260-1320°C in a reducing atmosphere, firing, and quenching. The invention enriches the types of existing black-glazed porcelain, and glazes once, with low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron-based black-glazed porcelain preparation, and particularly relates to a silver-glazed Jian tea bowl with earthworm crawling-in-mud patterns and a preparation method thereof. Background Art

[0002] Black-glazed porcelain was first produced in the Han Dynasty and developed in the Sui and Tang Dynasties. In the Song Dynasty, the popularity of the "tea-fighting" culture pushed the development of black-glazed porcelain technology to its peak, especially the black-glazed porcelain of Jian Kiln. Jian Kiln black-glazed porcelain products are rich in types, including black gold cups, rabbit hair cups, persimmon red cups, partridge spotted cups, and Yaobian oil-drop cups. Among them, the Yaobian oil-drop cup is called "the supreme divine product, a rare thing in the world, and a rare thing in ten thousand pieces."

[0003] Black-glazed porcelain is also considered to be an iron-based crystalline glaze porcelain. The types of iron oxide crystals are complex, and the color of the glaze surface is diversified with the addition of elements. Some scholars believe that the formation process of oil droplets is the separation of liquid phase in the glaze to produce small iron-rich droplets. The iron-rich droplets reach the glaze surface with the tiny bubbles generated by the reaction, and react with oxygen to form iron oxide crystal nuclei. The crystal nuclei absorb the iron elements in the glaze and continue to grow into iron oxide crystals until the glaze layer solidifies and the iron elements in the glaze cannot move. Deioie Colomban et al. found micron-sized ε-Fe2O3 crystals with a two-dimensional periodic arrangement structure in silver oil droplets, which can reflect the incident light with a mirror-like total reflection and present a silver-white metallic luster. Shi Xiaotao et al. studied modern imitation Yaobian oil droplets and found that the formation process of oil droplets is liquid phase separation, iron-rich phase moving to the glaze surface, nano-sized magnetite and hematite grains, thin crystal layer aggregation, and finally the bubbles burst on the glaze surface to form colored oil drop glaze. The coloring mechanism of oil-drop glaze is mainly due to the size and distribution density of the grains, which makes the wrinkled oil-drop spots have thin-film interference and grain scattering characteristics, thus producing iridescent structural colors. Although these studies reveal the formation process and coloring mechanism of black-glazed porcelain, there are no reports on the firing and analysis of silver-glazed Jianzhan with earthworm-walking mud patterns in the prior art.

[0004] The earthworm pattern appears on both Jun porcelain and celadon. The "earthworm pattern" on official Jun porcelain pieces from the Song Dynasty is formed during the drying or preheating stage of the glaze. It is caused by the evaporation of water in the glaze layer, which causes the glaze to shrink too much and form initial cracks. Then, during the firing process, it is filled with the most fusible components in the glaze. It is different from the flaking and cracking of the glaze surface of celadon and glazed components, which are caused by the different expansion coefficients of the body and glaze when the object cools. The earthworm pattern in black-glazed porcelain fired with two or three layers of glazing is an artistic effect caused by the flow of glazes of different compositions after firing. However, multi-layer glazing not only has high production costs and poor yields, but is also a huge waste of the increasingly dwindling raw material resources for ceramics. Summary of the invention

[0005] The invention provides a silver-glazed Jian tea bowl with earthworm-walking-in-mud patterns and a preparation method thereof, which enriches the types of existing black-glazed porcelain, and the glazing is performed once with low cost.

[0006] The present invention is achieved through the following technical solutions:

[0007] A method for preparing a silver-glazed Jianzhan with earthworm-walking mud patterns, comprising the following steps:

[0008] (1) preparing glaze raw materials into glaze; the glaze raw materials include: 50-70 parts of feldspar, 2-8 parts of kaolin, 15-25 parts of quartz, 10-16 parts of calcite, 0.5-2 parts of talc, 1-3 parts of tricalcium phosphate, 5-10 parts of boron frit, 0.1-0.6 parts of sodium tripolyphosphate, 0.5-1.5 parts of sodium carboxymethyl cellulose, 5-10 parts of ferric oxide, 1-2 parts of manganese dioxide, and 0.2-1 parts of cobalt oxide;

[0009] (2) dipping the green body into the glaze once for 10-20 seconds and drying;

[0010] (3) The dried green body is heated to 900°C in an oxidizing atmosphere, and to 1260-1320°C in a reducing atmosphere, fired, and rapidly cooled.

[0011] Preferably, step (1) specifically comprises: mixing the glaze raw material with ball stone, adding water for wet ball milling to make the glaze concentration reach 60%-65%, and passing through a 100-200 mesh sieve to obtain the glaze.

[0012] Furthermore, the wet ball milling adopts a rotation speed of 200-400 r / min and a time of 40-80 min.

[0013] Preferably, in step (3), the dried green body is heated to 900°C in an oxidizing atmosphere. Specifically, in an oxidizing atmosphere, the dried green body is heated to 600°C at a heating rate of 5°C / min, and then heated to 900°C at a heating rate of 3°C / min, and kept warm for 4-5h.

[0014] Preferably, in step (3), heating to 1260-1320° C. in a reducing atmosphere specifically comprises: heating to 1260-1320° C. in a reducing atmosphere at a heating rate of 1.5° C. / min.

[0015] Preferably, in step (3), the temperature is raised to 1260-1320°C in a reducing atmosphere, specifically: when the temperature is raised to 900°C, 300-600 parts of charcoal are added to the firing furnace and the temperature is raised to 1260-1320°C.

[0016] Preferably, in step (3), the firing time is 20-30 minutes.

[0017] Preferably, in step (3), the temperature is rapidly cooled to 1080-1050° C. and then naturally cooled to room temperature.

[0018] The silver-glazed Jian tea bowl with earthworm crawling in mud patterns is obtained by the preparation method.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The invention discloses a formula and a preparation method of a silver-glazed Jian tea bowl with earthworm crawling mud patterns. The silver-glazed Jian tea bowl with earthworm crawling mud patterns can be stably fired through a reasonable ratio and the preparation method. The invention adds manganese oxide, cobalt oxide and high-content ferric oxide to the raw materials, and the high-concentration ferric oxide is continuously decomposed into oxygen at high temperature in a reducing atmosphere, and small bubbles of oxygen are aggregated to gradually form large bubbles that rise and bring iron elements to the surface of the glaze layer. The iron elements gather near the bubbles and react with oxygen in the kiln in the cooling stage to form silver micron-sized ferric oxide particles, so that the glaze surface has a silver luster; the presence of cobalt oxide is conducive to the enrichment of iron oxide to form silver spots; the raw materials contain tricalcium phosphate, sodium tripolyphosphate and sodium hydroxymethyl cellulose, and the tricalcium phosphate promotes liquid phase separation, so that an emulsion phase is produced in the glaze, thereby increasing the wear resistance of the glaze; the sodium tripolyphosphate and sodium hydroxymethyl cellulose increase the viscosity of the glaze to adjust the fluidity and make it have good fluidity; during firing, the silver spots melt to form a liquid phase with a fine texture, and after being affected by gravity, they flow downward to expose the bottom black glaze, forming an iron-based black glaze pattern with natural and smooth lines hidden between the silver crystals, and shaped like a pattern of black earthworms walking in mud. The color spots of black-glazed porcelain in the prior art have poor fluidity and cannot flow to form earthworm patterns. The addition of cobalt oxide in the present invention also effectively improves the corrosion resistance and wear resistance of the glaze surface. A small amount of manganese oxide increases the blackness of the glass phase, and the glaze formed by the crystals on the surface also tends to be silvery white, making the silver-glazed Jianzhan with earthworm patterns have a higher gloss. After the blank of the present invention is fired, it is glazed once and fired once to form a pattern resembling earthworm patterns. The cost is low and the yield rate is above 75%. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a real picture of the silver-glazed Jian tea bowl with earthworm crawling mud pattern prepared in Example 1. DETAILED DESCRIPTION

[0022] In order to further understand the present invention, the present invention is described below in conjunction with embodiments. These descriptions are only to further explain the features and advantages of the present invention and are not intended to limit the claims of the present invention.

[0023] The silver-glazed Jian tea bowl with earthworm-walking mud pattern described in the present invention comprises, by mass fraction, 50-70 parts of feldspar, 2-8 parts of kaolin, 15-25 parts of quartz, 10-16 parts of calcite, 0.5-2 parts of talc, 1-3 parts of tricalcium phosphate, 5-10 parts of boron frit, 0.1-0.6 parts of sodium tripolyphosphate, 0.5-1.5 parts of sodium carboxymethyl cellulose, 5-10 parts of ferric oxide, 1-2 parts of manganese dioxide, and 0.2-1 parts of cobalt oxide.

[0024] The method for preparing the silver-glazed Jianzhan with earthworm-walking-in-mud patterns specifically comprises the following steps:

[0025] (1) Mix the raw materials of the glaze with 200 parts of ball stones of different particle sizes, add deionized water and mix with the raw materials for wet ball milling, keep the speed at 200-400 r / min for 40-80 min, so that the wet ball milling glaze concentration reaches 60%-65%, and sieve through 100-200 mesh to obtain silver glaze.

[0026] (2) The body is dipped in glaze only once, and the dipping time is 10-20 seconds and then dried at room temperature.

[0027] (3) The sintering temperature is 1260-1320°C, the holding time is 20-30 minutes, and the temperature is rapidly cooled to 1050°C and then cooled to room temperature along with the furnace.

[0028] In step (3), the specific firing system of the silver glaze Jianzhan includes the following steps:

[0029] 1) The dried body after glazing is placed in a kiln and fired in an oxidizing atmosphere at room temperature of 900°C for 4-5 hours. The heating rates from 25°C to 600°C to 900°C are 5°C / min and 3°C / min respectively.

[0030] 2) Firing from 900℃ to 1260-1320℃ must be carried out in a reducing atmosphere, and the heating rate is maintained at 1.5℃ / min; the insulation time at 1260-1320℃ is 20-30min.

[0031] 3) Rapidly cool to 1080-1050℃ and then cool to room temperature in the furnace.

[0032] The invention uses feldspar as the main solvent, the content of silicon dioxide in feldspar is 64.3%, aluminum oxide is 18.3%, potassium oxide is 12.9%, and the content of calcium oxide in calcite is 58.8%, which can not only reduce the melting temperature of the glaze, but also increase the alkalinity of the melting system and promote the crystallization of iron oxide. Quartz plays a skeleton role in ceramic glaze, and the phosphorus and calcium introduced by tricalcium phosphate can control the phase separation and produce an emulsification effect, thereby increasing the wear resistance of the glaze. The viscosity of the glaze adjusted by sodium tripolyphosphate and sodium carboxymethyl cellulose has good fluidity and ensures a round glaze surface. A high content of iron oxide is the key to producing silver glaze Jianzhan with earthworm mud patterns, and cobalt oxide and manganese dioxide additives enhance the glossiness of the silver glaze and the corrosion resistance of the glaze. The reasonable ratio of raw materials is very important for the color development of the glaze, and the firing process cannot be ignored. The firing system and atmosphere of the iron-based black glaze determine the color and pattern of the glaze. The silver-glazed Jianzhan with earthworm-like mud patterns prepared by changing the calcination atmosphere, holding time, rapid cooling process and raw material ratio enriches the existing Jianzhan types. The unique patterns and colors and the high yield rate increase the economic and artistic value of Jianzhan.

[0033] Example 1

[0034] The raw material formula of a silver-glazed Jian tea bowl with an earthworm-walking mud pattern: 53g feldspar, 2g kaolin, 15g quartz, 11g calcite, 1g talc, 2g commercial tricalcium phosphate, 10g boron frit, 0.3g sodium tripolyphosphate, 0.8g sodium carboxymethyl cellulose, 8.5g ferric oxide, 2g manganese dioxide, and 0.8g cobalt oxide.

[0035] The method for preparing the silver-glazed Jianzhan with earthworm-walking-in-mud patterns specifically comprises the following steps:

[0036] (1) The raw materials weighed according to the proportion are mixed with 200 g of ball stones of different particle sizes, and 80 ml of deionized water is added to the raw materials for wet ball milling. The speed is maintained at 400 r / min for 60 min, so that the wet ball milling glaze concentration reaches 65%, and the silver glaze is obtained by sieving through 150 mesh.

[0037] (2) The body is dipped in glaze only once, and the dipping time is 10 seconds and then dried at room temperature.

[0038] (3) After glazing, the dried body is placed in a kiln and fired in an oxidizing atmosphere at room temperature of 900°C for 4 h. The heating rates from 25°C to 600°C to 900°C are 5°C / min and 3°C / min, respectively.

[0039] (4) Firing at 900-1280℃ must be carried out in a reducing atmosphere. When the furnace temperature reaches 900℃, remove the plug and add 400g of charcoal to ensure reducing flame firing. The heating rate is maintained at 1.5℃ / min; the insulation time at 1280℃ is 30min.

[0040] (5) Rapidly cool to 1050°C and then cool to room temperature in the furnace.

[0041] The actual picture of the silver-glazed Jianzhan with earthworm-walking mud pattern described in this embodiment is as follows: Figure 1 As shown, obvious earthworm patterns can be seen.

[0042] Example 2

[0043] The raw material formula of a silver-glazed Jian teak with an earthworm walking in mud pattern: 55g feldspar, 2g kaolin, 13g quartz, 11g calcite, 1.5g talc, 2g commercial tricalcium phosphate, 10g boron frit, 0.3g sodium tripolyphosphate, 0.8g sodium carboxymethyl cellulose, 8g ferric oxide, 2g manganese dioxide, and 1g cobalt oxide.

[0044] The method for preparing the silver-glazed Jianzhan with earthworm-walking-in-mud patterns specifically comprises the following steps:

[0045] (1) The raw materials weighed according to the proportion are mixed with 200 g of ball stones of different particle sizes, and 80 ml of deionized water is added to the raw materials for wet ball milling. The speed is maintained at 2000 r / min for 80 min, so that the wet ball milling glaze concentration reaches 60%, and the silver glaze is obtained by sieving through 150 mesh.

[0046] (2) The body is dipped in glaze only once, and the dipping time is 10 seconds and then dried at room temperature.

[0047] (3) After glazing and drying, the green body is placed in a kiln and fired in an oxidizing atmosphere at room temperature of 900°C for 4 h. The heating rates from 25°C to 600°C to 900°C are 5°C / min and 3°C / min, respectively.

[0048] (4) Firing at 900-1280℃ must be carried out in a reducing atmosphere. When the furnace temperature reaches 900℃, remove the plug and add 400g of charcoal to ensure reducing flame firing. The heating rate is maintained at 1.5℃ / min; the insulation time at 1280℃ is 30min.

[0049] (5) Rapidly cool to 1050°C and then cool to room temperature in the furnace.

[0050] The silver-glazed Jian teak, prepared by reasonable proportion of glaze formula and controlling the atmosphere and temperature of the overall firing process, is bright white in color, with a unique decorative effect of black earthworm patterns, natural and vivid lines, and high glaze strength.

[0051] Example 3

[0052] The raw material formula of a silver-glazed Jian teak with an earthworm-walking mud pattern: 53g feldspar, 2g kaolin, 15g quartz, 11g calcite, 1.5g talc, 2g commercial tricalcium phosphate, 10g boron frit, 0.3g sodium tripolyphosphate, 0.8g sodium carboxymethyl cellulose, 8g ferric oxide, 2g manganese dioxide, and 0.5g cobalt oxide.

[0053] The preparation method of the silver-glazed Jianzhan with earthworm-walking mud patterns specifically comprises the following steps:

[0054] (1) The raw materials weighed according to the proportion are mixed with 200 g of ball stones of different particle sizes, and 80 ml of deionized water is added to the raw materials for wet ball milling. The speed is maintained at 400 r / min for 40 min, so that the wet ball milling glaze concentration reaches 63%. The glaze is sieved through 120 mesh to obtain a silver glaze.

[0055] (2) The body is dipped in glaze only once, and the dipping time is 20 seconds and then dried at room temperature.

[0056] (3) After glazing and drying, the green body is placed in a kiln and fired in an oxidizing atmosphere at room temperature of 900°C for 4 h. The heating rates from 25°C to 600°C to 900°C are 5°C / min and 3°C / min, respectively.

[0057] (2) Firing at 900-1280℃ must be carried out in a reducing atmosphere. When the furnace temperature reaches 900℃, remove the plug and add 400g of charcoal to ensure reducing flame firing. The heating rate is maintained at 1.5℃ / min; the insulation time at 1280℃ is 30min.

[0058] (3) Rapidly cool to 1050°C and then cool to room temperature in the furnace.

[0059] By adjusting the content of cobalt oxide in the formula, it is shown that cobalt oxide plays an important role in glaze. The atmosphere and temperature of the whole firing process remain unchanged, but the dipping time is extended during glazing to ensure the thickness of the glaze, so that enough iron oxide is precipitated during calcination to make the glaze surface silver, and less cobalt oxide makes the glaze surface silver-gray (that is, silver-white crystals are precipitated in the black glaze). The thicker glaze layer enhances fluidity, deepens the color of the bottom black glaze in a reducing atmosphere, and the artistic effect of earthworm mud patterns becomes more obvious.

[0060] Comparative Example 1

[0061] The raw material formula of a silver-glazed Jian teak with an earthworm-walking mud pattern: 33g feldspar, 43g purple clay, 15g quartz, 11g calcite, 1.5g talc, 2g commercial tricalcium phosphate, 10g boron frit, 0.3 sodium tripolyphosphate, 0.8g sodium carboxymethyl cellulose, 2g manganese dioxide, and 1g cobalt oxide.

[0062] The preparation method is the same as that of Example 2. The glaze prepared by combining a small amount of feldspar with high iron content to replace iron oxide and kaolin has a large viscosity. The fluidity of the glaze after high-temperature calcination is poor, and only part of the iron oxide crystals are precipitated. Although this method is conducive to the waste utilization of purple clay tailings resources, the fired product has large defects and does not have high artistic value and economic value. The appropriate addition of iron oxide and the viscosity of the glaze are closely related to the yield of the product.

[0063] Comparative Example 2

[0064] The raw material formula of a silver-glazed Jian teak with an earthworm-walking mud pattern: 53g feldspar, 2g kaolin, 15g quartz, 11g calcite, 1.5g talc, 2g commercial tricalcium phosphate, 10g boron frit, 0.3 sodium tripolyphosphate, 0.8g sodium carboxymethyl cellulose, 8g ferric oxide, 2g manganese dioxide, and 1g cobalt oxide.

[0065] The preparation method is the same as that in Example 2, but pure oxidizing atmosphere and over-reducing atmosphere are used for firing respectively. When firing in an oxidizing atmosphere, the ferric oxide decomposes into iron and oxygen after the glaze is completely melted. Under the oxidizing atmosphere, the decomposed iron element is completely oxidized after contacting with the air in the kiln, and the surface of the glaze is all white and crystallized to be silvery white. Firing in a reducing atmosphere will cause the iron oxide to be reduced to iron element and exist in the glaze, making the glaze surface completely black. The Jianzhan does not have the silver glaze decoration with earthworm patterns or is all black glaze. This shows that a partial reducing atmosphere must be used in the furnace, and proper control is required to obtain the silver glaze Jianzhan with earthworm patterns.

[0066] Comparative Example 3

[0067] The raw material formula of a silver-glazed Jian teak with an earthworm-walking mud pattern: 53g feldspar, 2g kaolin, 15g quartz, 11g calcite, 1.5g talc, 2g commercial tricalcium phosphate, 10g boron frit, 0.3 sodium tripolyphosphate, 0.8g sodium carboxymethyl cellulose, 8g ferric oxide, 2g manganese dioxide, and 1g cobalt oxide.

[0068] The preparation method is the same as that of Example 2, but there is no quenching treatment during the cooling process. The glaze surface of the Jianzhan prepared in this way is rough and has poor glossiness. The precipitated silver spots are small and cannot be combined with the bottom black glaze to form an artistic glaze surface with earthworm mud patterns. When preparing silver-glazed Jianzhan, the quenching process can ensure that a large number of silver spots are precipitated on the glaze surface and do not merge with each other, which produces a complementary effect with the bottom black glaze.

[0069] The formula of the silver-glazed Jianzhan with earthworm-walking mud pattern provided in Example 4-23 of the present invention is shown in Table 1-4, with the unit being g. The preparation method thereof is the same as that in Example 2.

[0070] Table 1 Raw material formula of Examples 4-8

[0071] raw material Example 4 Example 5 Example 6 Example 7 Example 8 Feldspar 50 55 60 65 70 Calcite 11 12 10 10 12 quartz 15 15 15 10 10 Kaolin 2 4 2 1 2 talc 0.5 0.8 1 0.5 1 Tricalcium phosphate 1 2 1 2 2 Boron Frit 10 8 7 6 5 Sodium tripolyphosphate 0.1 0.3 0.3 0.3 0.1 Sodium Carboxymethyl Cellulose 0.5 0.8 0.8 0.8 0.5 Iron (III) oxide 7.5 8 7 6 7.5 Manganese dioxide 1.5 1.5 2 1 1 Cobalt Oxide 1 0.4 0.5 0.5 0.5

[0072] Table 2 Raw material formula of Examples 9-13

[0073] raw material Example 9 Example 10 Embodiment 11 Example 12 Embodiment 13 Feldspar 50 60 65 55 50 Calcite 10 10 10 10 13 quartz 15 15 13 15 20 Kaolin 2 1 6 1 2 talc 1 0.5 2 0.5 1.5 Tricalcium phosphate 1 2 1.5 2 1 Boron Frit 5 7 6 6 8 Sodium tripolyphosphate 0.6 0.4 0.3 0.5 0.1 Sodium Carboxymethyl Cellulose 1.5 1.1 0.8 1.2 0.3 Iron (III) oxide 10 7 8 6 9 Manganese dioxide 1 2 0.5 1 2 Cobalt Oxide 0.5 1 0.2 0.5 1

[0074] Table 3 Raw material formula of Examples 14-18

[0075] raw material Embodiment 14 Embodiment 15 Example 16 Embodiment 17 Embodiment 18 Feldspar 55 60 70 65 60 Calcite 14 11 12 10 13 quartz 25 20 15 15 15 Kaolin 2 1.5 1 1 2 talc 1.5 1 1 1 1 Tricalcium phosphate 1 2 1 2 1 Boron Frit 10 6 5 6 7 Sodium tripolyphosphate 0.1 0.4 0.2 0.5 0.3 Sodium Carboxymethyl Cellulose 0.3 1 0.5 1.2 0.8 Iron (III) oxide 8 7 6.5 6 8 Manganese dioxide 2 1.5 2 1 1.5 Cobalt Oxide 1 0.5 0.5 0.5 0.5

[0076] Table 4 Raw material formula of Examples 19-23

[0077] raw material Embodiment 19 Embodiment 20 Embodiment 21 Embodiment 22 Embodiment 23 Feldspar 70 50 60 55 65 Calcite 10 14 12 16 11 quartz 15 20 18 20 15 Kaolin 2 4 2 2 2 talc 1 1 1.5 1.8 1 Tricalcium phosphate 2 1 2 1.5 2 Boron Frit 5 8 4 7 10 Sodium tripolyphosphate 0.3 0.2 0.7 0.4 0.3 Sodium Carboxymethyl Cellulose 0.8 0.6 1.5 1 0.8 Iron (III) oxide 7.5 9 7 9 8.5 Manganese dioxide 1 2 1 2 2 Cobalt Oxide 0.5 1 0.5 1 1.5

[0078] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a silver-glazed Jianzhan with earthworm-walking mud patterns, characterized in that: The following steps are involved: (1) preparing glaze raw materials into glaze; the glaze raw materials include, by weight: 50-70 parts of feldspar, 2-8 parts of kaolin, 15-25 parts of quartz, 10-16 parts of calcite, 0.5-2 parts of talc, 1-3 parts of tricalcium phosphate, 5-10 parts of boron frit, 0.1-0.6 parts of sodium tripolyphosphate, 0.5-1.5 parts of sodium carboxymethyl cellulose, 5-10 parts of ferric oxide, 1-2 parts of manganese dioxide, and 0.2-1 parts of cobalt oxide; (2) dipping the green body into the glaze once for 10-20 seconds and drying; (3) In an oxidizing atmosphere, heat the dried body to 600°C at a heating rate of 5°C / min, then heat it to 900°C at a heating rate of 3°C / min, keep it at that temperature for 4-5h, heat it to 1260-1320°C at a heating rate of 1.5°C / min in a reducing atmosphere, fire it for 20-30min, cool it to 1080-1050°C, and then cool it naturally to room temperature.

2. The method for preparing the silver-glazed Jianzhan with earthworm-walking-in-mud patterns according to claim 1, characterized in that: Step (1) specifically comprises: mixing the glaze raw material with ball stone, adding water for wet ball milling to make the glaze concentration reach 60%-65%, and passing through a 100-200 mesh sieve to obtain a glaze.

3. The method for preparing the silver-glazed Jianzhan with earthworm-walking-in-mud patterns according to claim 2, characterized in that: The speed of wet ball milling is 200-400r / min and the time is 40-80min.

4. The method for preparing the silver-glazed Jianzhan with earthworm-walking-in-mud patterns according to claim 1, characterized in that: In step (3), the temperature is raised to 1260-1320°C in a reducing atmosphere. Specifically, when the temperature is raised to 900°C, 300-600 parts of charcoal are added into the firing furnace and the temperature is raised to 1260-1320°C.

5. A silver-glazed Jian ware with earthworm crawling patterns obtained by the preparation method described in any one of claims 1 to 4.

Citation Information

Patent Citations

  • Medium- and low-temperature fast firing glaze with silver spot effect and application thereof

    CN113912295A

  • Silver glaze and preparation method for firing silver glaze in reducing atmosphere

    CN115838246A