Growth methods and equipment for preparing high-quality silicon carbide crystals
By employing a two-stage crystal growth method and a silicon carbide crystal growth device with a dual-crucible design, the problems of dislocations and microtube defects in the PVT method were solved, and the growth of high-quality silicon carbide crystals was achieved.
Patent Information
- Application Number
- CN202310474685.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-04-27
AI Technical Summary
In existing technologies, microscopic defects such as dislocations and microtubes are prone to occur during the growth of silicon carbide crystals using the PVT method, leading to a decline in crystal quality.
A two-stage crystal growth method is adopted. First, the microtube defects of the seed crystal are eliminated in the silicon carbide melt by the Czochralski method. Then, the crystal is grown by the gas phase method. At the same time, a double crucible design and a flow guiding device are used to control the gas flow to ensure the uniformity of the crystal growth environment.
This effectively reduces dislocations and microtube defects in the seed crystal, improves the quality and grade of silicon carbide crystals, and ensures the uniformity and purity of crystal growth.
Smart Images

Figure CN116536766B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor technology, and in particular to a method and apparatus for preparing high-quality silicon carbide crystals. Background Technology
[0002] The related technology points out that the PVT method is one of the most commonly used methods for growing silicon carbide crystals. During the growth process using the PVT method, microscopic defects such as dislocations and microtubes are prone to appear in the crystal. Since these defects can be inherited during the crystal growth process, they directly lead to a decrease in crystal quality. Summary of the Invention
[0003] The present invention aims to at least solve one of the technical problems existing in the prior art. To this end, the present invention proposes a growth method for preparing high-quality silicon carbide crystals, which can reduce defects such as dislocations and microtubes in the crystal and improve the crystal quality.
[0004] The present invention also proposes a growth apparatus based on the above-described growth method for preparing high-quality silicon carbide crystals.
[0005] The method for preparing high-quality silicon carbide crystals according to a first aspect of the present invention includes: 1) First crystal growth stage: The first crystal growth stage uses the Czochralski method to grow silicon carbide seed crystals by immersing the silicon carbide seed crystals in molten silicon carbide to eliminate microtube defects in the seed crystals. 2) Second crystal growth stage: The second stage uses a vapor phase method to grow silicon carbide seed crystals obtained in step 1).
[0006] The above scheme employs two crystal growth stages. In the first stage, a silicon carbide seed crystal is immersed in molten silicon carbide and grown using the Czochralski method, eliminating microtubule defects and dislocations in the seed crystal. In the second stage, a vapor phase method is used to grow the silicon carbide seed crystal after eliminating microtubule defects. This method effectively reduces inherited dislocations in the seed crystal, thereby improving crystal quality.
[0007] According to a second aspect of the present invention, a growth apparatus for preparing high-quality silicon carbide crystals includes an outer crucible, a melting chamber, an inner crucible, a flow guiding device, a rotary lifting shaft, a seed crystal holder, and a transmission device. The outer crucible is sealed with a crucible lid, defining a first space. The melting chamber is disposed on the inner bottom wall of the outer crucible, and has an opening at its upper part. The lid is installed on the top of the melting chamber. The inner crucible is installed inside the melting chamber. The flow guiding device is connected to the inner wall of the outer crucible. The top end of the rotary lifting shaft is located outside the outer crucible and connected to an external rotary lifting device, while the bottom end of the rotary lifting shaft is located inside the outer crucible. The rotary lifting shaft is coaxially arranged with the inner crucible. The seed crystal holder is installed at the bottom of the rotary lifting shaft, and a seed crystal is mounted on its lower surface. The transmission device is connected to the rotary lifting shaft via a connecting component. The transmission device controls the lid to close as the rotary lifting shaft rises, and controls the flow guiding device to close as the rotary lifting shaft rises. After the flow guiding device closes, it divides the first space into a growth space and a raw material space.
[0008] In the above scheme, the present invention adopts a double crucible design. The inner crucible is used to load the Si-C source, and the outer crucible is used to load the silicon carbide powder. Before crystal growth, the silicon carbide seed crystal is first placed inside the inner crucible. The initial state of the present invention is as follows: the inner crucible is fixed in a preset position in the melting chamber, the flow guiding device is in the open state, and the rotating lifting shaft passes through the flow guiding device to place the silicon carbide seed crystal inside the inner crucible. The first crystal growth stage is carried out first. The molten Si-C melt is used to repair the dislocations and microtube defects on the seed crystal. After the repair is completed, the seed crystal is gradually lifted by the rotating lifting shaft. During the rise of the seed crystal, the transmission device drives the cover and the flow guiding device to slowly close as the rotating lifting shaft rises. When the silicon carbide seed crystal rises to the preset position with the rotating lifting shaft, the cover and the flow guiding device are completely closed. At this time, the crystal enters the second crystal growth stage. Since the microtubes and dislocations of the silicon carbide seed crystal have been repaired, the microtubes and dislocations will not reappear during the subsequent crystal growth process, effectively improving the quality of the silicon carbide crystal.
[0009] In addition, since the only power source for the closure of the flow guiding device and the descent of the inner crucible is the rising of the rotating lifting shaft, it effectively ensures that there is no excessive disturbance in the growth space, thereby further ensuring the quality of silicon carbide crystals.
[0010] In some embodiments, the flow guiding device of the present invention includes an annular flow guiding platform and a flow guiding plate. The annular flow guiding platform is connected to the inner wall of the outer crucible. A flow guiding hole is defined in the middle of the annular flow guiding platform, and the seed crystal holder can pass through the flow guiding hole as the rotating lifting shaft moves up and down. The flow guiding plate is connected to the annular flow guiding platform through a first rotating shaft. The first rotating shaft can drive the flow guiding plate to rotate under the action of the transmission device and form a shielding on the flow guiding hole to close the flow guiding device.
[0011] In some embodiments, the guide plate of the present invention consists of four quarter-circle perforated plates. Each perforated plate is connected to the annular guide platform via a first rotating shaft. The first rotating shaft is connected to the rotating lifting shaft via the transmission device. When the rotating lifting shaft rises to a preset position, the transmission shaft drives the perforated plate to rotate and close into the guide plate via the first rotating shaft, thus blocking the guide holes and closing the guide device. In this embodiment, the rotating lifting shaft controls the operation of the transmission device, which in turn drives the first rotating shaft to rotate, thereby causing the perforated plate to rotate and close into the guide plate, thus closing the guide device. This control method does not interfere with the silicon carbide gas, thus avoiding any impact on the quality of the silicon carbide crystal. Furthermore, after the perforated plate blocks the guide holes, the silicon carbide gas entering the growth space after passing through the perforated plate is more uniform, which is beneficial to improving the growth quality of the crystal.
[0012] In some embodiments, the cover of the present invention is a double-door structure composed of two cover plates, each door plate being connected to the side wall of the melting chamber via a hinge; the inner crucible is fixed to the bottom wall inside the melting chamber via the telescopic support frame, and the inner crucible descends into the melting chamber as the rotating lifting shaft rises under the pull of the transmission device; in this embodiment, when the rotating lifting shaft rises, it drives the transmission device to move, and the transmission device in turn drives the inner crucible to descend. When the inner crucible descends, the cover automatically closes under the action of the hinge and its own gravity, thereby realizing the control of the inner crucible descending into the melting chamber through a purely mechanical means, while automatically closing the cover, thus avoiding any impact on the quality of the crystal.
[0013] In some embodiments, the transmission device of the present invention includes a first traction line and a second traction line. One end of each first traction line is connected to the connecting component, and the other end passes sequentially through the crucible cover and the side wall and bottom wall of the outer crucible, and is fixed to the bottom of the inner crucible. The first traction line pulls the inner crucible downward as the rotating lifting shaft rises. One end of each second traction line is connected to the connecting component, and the other end passes sequentially through the crucible cover, the side wall of the outer crucible, and the side wall of the annular guide platform, and is wound in the same direction around the lower part of the first rotating shaft. As the rotating lifting shaft rises, the second traction line drives the perforated plate to rotate and close into the guide plate through the first rotating shaft. The number of both the first and second traction lines is four, and they are evenly spaced in the circumferential direction. In this embodiment, the traction lines control the closure of the perforated plate to close the guide device, and simultaneously control the descent of the inner crucible into the melting chamber to close the cover. The control method is simple, convenient, and low in cost.
[0014] In some embodiments, the transmission device of the present invention further includes a traction wire transmission channel, which mainly consists of a first traction wire transmission channel, a second traction wire transmission channel, and a third traction wire transmission channel; the first traction wire transmission channel is defined within the crucible cover, the second traction wire transmission channel is defined within the outer crucible wall, and the third traction wire transmission channel is defined within the side wall of the annular guide platform; wherein, one end of the first traction wire transmission channel communicates with the shaft hole of the rotating lifting shaft, and the other end communicates with one end of the second traction wire transmission channel, the other end of the second traction wire transmission channel communicates with the bottom of the melting chamber, and the third traction wire transmission channel... One end of the guide is connected to the shaft hole of the first rotating shaft, and the other end is connected to the second traction wire transmission channel. Four traction wire transmission channels are provided, evenly spaced in the circumferential direction, with each shaft hole of the first rotating shaft corresponding to one traction wire transmission channel. One end of the first traction wire is connected to the bottom of the inner crucible, and the other end passes through the second traction wire transmission channel and the first traction wire transmission channel sequentially, connecting to the connecting component. One end of the second traction wire is wound around the first rotating shaft, and the other end passes through the third traction wire transmission channel, the second traction wire transmission channel, and the first traction wire transmission channel sequentially, connecting to the connecting component. In this embodiment, traction wire transmission channels are provided. One end of the first and second traction wires is connected to the connecting component, and the other ends of the first and second traction wires pass through the traction wire transmission channels and are connected to the first rotating shaft and the bottom of the inner crucible, respectively. Because the traction wire transmission channels define a space to accommodate the traction wires, the friction between the traction wires and the outer crucible wall and the crucible lid wall during movement is reduced, extending the service life of the traction wires and making the transmission smoother.
[0015] In some embodiments, the connecting component of the present invention is a connecting ring or a bearing. An annular groove is formed on the side wall of the rotary lifting shaft. The connecting ring or bearing is sleeved on the rotary lifting shaft and placed within the annular groove. The outer diameter of the connecting ring or bearing is not greater than the outer diameter of the rotary lifting shaft. When the connecting component is a connecting ring, the connecting ring and the rotary lifting shaft are clearance-fitted, and the contact surfaces of the connecting ring and the rotary lifting shaft are both polished surfaces. The transmission device is fixedly connected to the connecting ring. When the connecting component is a bearing, the inner ring of the bearing is interference-fitted with the rotary lifting shaft, and the transmission device is fixedly connected to the outer ring of the bearing.
[0016] In some embodiments, the inner crucible of the present invention is fixedly installed on the upper side of the melting chamber. The cover is composed of four quarter-circle cover plates, each of which is connected to the top of the side wall of the melting chamber via a second rotating shaft. The second rotating shaft, under the action of a transmission device, controls the opening or closing of the cover by rotating the lifting shaft. In this embodiment, the position of the inner crucible is fixed, and the cover plates are opened or closed by rotation.
[0017] In some embodiments, the connecting part of the present invention is a rack, which is disposed on the outer wall of the rotating lifting shaft. The transmission device includes a traction shaft and a gear. The traction shaft includes a first traction shaft, a second traction shaft, a third traction shaft, a fourth traction shaft, and a fifth traction shaft. One end of the first traction shaft meshes with the rack via a gear. The other end of the first traction shaft is connected to one end of the third traction shaft via the second traction shaft. The other end of the third traction shaft is connected to the first rotating shaft. One end of the third traction shaft is connected to one end of the fifth traction shaft via the fourth traction shaft. The other end of the fifth traction shaft is connected to the second rotating shaft. The first traction shaft and the second traction shaft, the second traction shaft and the third traction shaft, the third traction shaft and the first rotating shaft, the third traction shaft and the fourth traction shaft, the fourth traction shaft and the fifth traction shaft, and the fifth traction shaft and the second rotating shaft are all connected by bevel gear pairs. A total of four traction shafts are provided and are evenly spaced in the circumferential direction. In this embodiment, as the rotating lifting shaft rises, the seed crystal rises and passes through the guide hole. At the same time, the meshing transmission of the gear and rack, as well as the bevel gear pairs between each traction shaft, drives the perforated plate and cover plate to rotate slowly inward. When the rotating lifting shaft rises to the preset position, the perforated plate and cover plate are completely closed or opened, that is, the annular guide platform and cover are closed. This realizes that the closure or opening of the annular guide platform and cover can be controlled by only the rise of the rotating lifting shaft, thus avoiding any impact on the growth quality of the crystal.
[0018] In some embodiments, the present invention further includes a traction shaft drive channel, wherein the traction shaft is mounted within the traction shaft drive channel via a retaining ring, and the traction shaft and the retaining ring are clearance-fitted; the traction shaft drive channel includes a first traction shaft drive channel, a second traction shaft drive channel, and a third traction shaft drive channel, wherein the first traction shaft drive channel is defined within the crucible cover, the second traction shaft drive channel is defined within the outer crucible sidewall, and the third traction shaft drive channel is defined within the annular guide platform sidewall; one end of the first traction shaft drive channel communicates with the shaft hole of the rotary lifting shaft, and the other end communicates with one end of the second traction shaft drive channel. One end of the third traction shaft transmission channel is connected to the shaft hole of the first rotating shaft, and the other end is connected to the second traction shaft transmission channel. The number of traction shaft transmission channels is the same as the number of the first rotating shafts, and each shaft hole of the first rotating shaft corresponds to one traction shaft transmission channel. The first traction shaft and the second traction shaft are respectively placed in the first traction shaft transmission channel and the second traction shaft transmission channel. The third traction shaft and the fourth traction shaft are arranged vertically within the second traction shaft transmission channel, and each first rotating shaft corresponds to one traction shaft transmission channel. A total of four traction shaft transmission channels are provided, and they are evenly spaced in the circumferential direction. In this embodiment, the traction shaft channels can accommodate the traction shafts, reducing friction between the traction shafts and the crucible cover, outer crucible wall, and sidewall of the annular guide platform during rotation, thus extending the service life of the traction shafts.
[0019] Compared with the prior art, the present invention has the following advantages: 1) The crucible of this invention mainly contains silicon material and carbon powder. In the second crystal growth stage, the silicon material and carbon powder react continuously to generate SiC. The SiC decomposes upon heating to generate Si2C, SiC2, and Si gas. After the gas rises, it mixes with the silicon carbide gas after the sublimation of the surrounding silicon carbide powder, which increases the silicon vapor content in the mixed gas. The excess silicon vapor can react with carbon particles in the air, thereby reducing the carbon content in the gas, which in turn reduces impurities such as carbon inclusions and improves the crystal quality. The mixed gas passes through a closed porous plate, which can play a role in homogenizing the airflow and further improve the growth quality of the crystal.
[0020] 2) During the heating process, the heat is mainly generated through the crucible, and then the heat is conducted to the silicon carbide powder. This results in the temperature of the silicon carbide powder near the crucible being higher than that far from the crucible. Therefore, this invention adopts an inner and outer crucible design, in which the inner and outer crucible walls heat the silicon carbide powder simultaneously, making the powder more uniformly heated and avoiding the problem of uneven heating of the powder during the heating process affecting crystal growth.
[0021] 3) During crystal growth, in addition to the need for uniform heat in the silicon carbide powder, the temperature at the crystal also needs to be uniform. Uneven temperature distribution will increase crystal stress, which is the main source of micro-defects such as MP, BPD, and TED. This invention, due to the presence of the inner crucible, increases the intermediate heat. The seed crystal can receive heat conduction from the outer crucible and also heat radiation from the inner crucible below, making its radial temperature gradient more uniform, reducing stress, and improving the crystal growth quality.
[0022] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description
[0023] Figure 1 This is a schematic diagram of a structure for a high-quality silicon carbide crystal growth apparatus according to an embodiment of the present invention; Figure 2 This is a schematic diagram of a structure for a high-quality silicon carbide crystal growth apparatus according to an embodiment of the present invention; Figure 3 This is a schematic diagram of the rotating and closing process of a porous plate in a high-quality silicon carbide crystal growth apparatus according to an embodiment of the present invention; wherein, Figure (a) shows the guide plate in a fully open state, Figures (b) and (c) show the guide plate in a semi-closed state, and Figure (d) shows the guide plate in a fully closed state; Figure 4 This is a schematic diagram of the process of the inner crucible descending to the melting chamber and the cover closing in a high-quality silicon carbide crystal growth apparatus according to an embodiment of the present invention; wherein, Figure (a) shows the cover fully open, Figure (b) shows the cover in a semi-closed state, and Figure (c) shows the cover fully closed. Figure 5 This is a schematic diagram of a structure for a high-quality silicon carbide crystal growth apparatus according to an embodiment of the present invention; Figure 6 yes Figure 2 This is a schematic diagram of the lifting and rotating shaft structure of a high-quality silicon carbide crystal growth apparatus according to an embodiment of the present invention; Figure 7 This is an enlarged structural schematic diagram of a high-quality silicon carbide crystal growth apparatus according to an embodiment of the present invention, showing that the first traction shaft and the second traction shaft are connected together by a bevel gear pair. Figure label: 100: Silicon carbide crystal growth equipment; 10: Thermal insulation cotton; 20: Crucible lid; 30: Outer crucible; 31: Silicon carbide powder; 40: Flow guiding device; 41: Annular flow guiding platform; 42: Flow guiding plate; 421: Perforated plate; 43: First rotating shaft; 44: Flow guiding hole; 50: Telescopic support frame; 60: Melting chamber; 61: Cover; 611: Cover plate; 62: Inner crucible; 70: Seed crystal holder; 71: Seed crystal; 80: Rotary lifting shaft; 81: Connecting ring; 91: First traction line drive channel; 92: Second traction line drive channel; 921: First traction line; 93: Third traction line drive channel; 931: Second traction line; 94: Retaining ring; 95: Rack; 961: First traction shaft drive channel; 962: Second traction shaft drive channel; 963: Third traction shaft drive channel; 971: First traction shaft; 972: Second traction shaft; 973: Third traction shaft; 974: Fourth traction shaft; 975: Fifth traction shaft; 98: Bevel gear pair. Detailed Implementation
[0024] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0025] The following disclosure provides numerous different embodiments or examples for implementing various structures of the invention. To simplify the disclosure, specific examples of components and arrangements are described below. These are merely examples and are not intended to limit the invention. Furthermore, reference numerals and / or letters may be repeated in different examples. Such repetition is for simplification and clarity and does not in itself indicate a relationship between the various embodiments and / or arrangements discussed. Additionally, examples of various specific processes and materials are provided in this invention; however, those skilled in the art will recognize the applicability of other processes and / or the use of other materials.
[0026] Example 1 According to an embodiment of the present invention, a method for preparing high-quality silicon carbide crystals is provided. The present invention employs a two-stage crystal growth process, the specific method of which is as follows: 1) First crystal growth stage: The silicon carbide seed crystal 71 is immersed in high-temperature silicon carbide melt, and the seed crystal 71 is grown using the Czochralski method. The atoms in the melt will compensate for the micro-defects and dislocations in the silicon carbide seed crystal 71, causing the threading screw dislocations (TSDs) or threading edge dislocations (TEDs) in the crystal to be transformed into stacking faults (SFs) during the growth process, changing their propagation direction, and finally being discharged outside the crystal. This achieves a decrease in the dislocation density in the grown crystal, thereby obtaining a high-quality SiC crystal (silicon carbide crystal) with no microtubes and low dislocation density. After the micro-defects of the seed crystal 71 are eliminated, the second crystal growth stage is carried out.
[0027] 2) Second crystal growth stage: The silicon carbide seed crystal 71 obtained in step 1) after eliminating microtube defects and dislocations is grown by vapor phase method. This method can reduce the inherited dislocations in the seed crystal 71, thereby improving the crystal quality.
[0028] Example 2 The following is for reference. Figures 1-4 A silicon carbide crystal growth apparatus 100 based on the above-described growth method is described, comprising an outer crucible 30, a melting chamber 60, a cover 61, an inner crucible 62, a flow guiding device 40, a rotary lifting shaft 80, a seed crystal holder 70, and a transmission device. The outer crucible 30 is surrounded by insulating cotton 10 to maintain the temperature inside. A crucible cover 20 is sealed on the top of the outer crucible 30, defining a first space. The melting chamber 60 is located on the inner bottom wall of the outer crucible 30 and has an opening at its upper part. The melting chamber 60 has a cylindrical structure and is made of graphite. The cover 61 is installed on the top of the melting chamber 60 to cover the opening above it. The inner crucible 62 is installed inside the melting chamber 60 and is mainly used to hold silicon material and carbon powder. The flow guiding device... 40 is connected to the inner wall of the outer crucible 30, which serves as a guide for the silicon carbide gas. The top end of the rotating lifting shaft 80 is located outside the outer crucible 30 and connected to the external rotating lifting device. The bottom end of the rotating lifting shaft 80 is located inside the outer crucible 30. The rotating lifting shaft 80 is coaxially arranged with the inner crucible 62. The seed crystal holder 70 is installed at the bottom of the rotating lifting shaft 80, and a seed crystal 71 is installed on its lower surface. The transmission device is connected to the rotating lifting shaft 80 through a connecting component. As the rotating lifting shaft 80 rises, the transmission device controls the cover 61 and the flow guiding device 40 to close slowly. After the flow guiding device 40 closes, it divides the first space into a growth space and a raw material space. The growth space is located in the upper part of the first space and is used for silicon carbide crystal growth. The raw material space is located in the lower part of the first space and is used to hold silicon carbide powder.
[0029] For details, please refer to Figure 1As shown, in this embodiment, an outer crucible 30, a melting chamber 60, and an inner crucible 62 are coaxially arranged from the outside to the inside. A flow guiding device 40 is connected to the inner wall of the outer crucible 30. The flow guiding device 40 and the cover 61 have two states: open and closed. The initial state of the flow guiding device 40 and the cover 61 is the open state. The rotating lifting shaft 80 passes through the flow guiding device 40 to place the seed crystal 71 inside the inner crucible 62. Si powder and C powder are placed in the inner crucible 62, and silicon carbide powder 31 is placed in the raw material space.
[0030] The equipment is started, and the first crystal growth stage is carried out by raising the temperature to 1500-1700℃. The silicon carbide crystal grows inside the inner crucible 62, and the dislocations and microtubes on the seed crystal 71 are repaired by using the molten Si-C melt. The silicon carbide crystal grows in the inner crucible 62 using the Czochralski method. The first crystal growth stage in the inner crucible 62 lasts for 10 hours. During the 10 hours, the rotating lifting shaft 80 pulls the seed crystal 71 upward at a speed of 0.05 mm / h. That is, the rotating lifting shaft 80 pulls the seed crystal 71 upward while rotating it. Due to the presence of the connecting parts, when the rotating lifting shaft 80 rotates, the connecting parts do not rotate with it. Therefore, it does not drive the transmission device, and thus does not drive the cover 61 and the flow guiding device 40 to move. However, when the rotating lifting shaft 80 moves axially, it can drive the transmission device to move, and then the transmission device drives the cover 61 and the flow guiding device 40 to close. After the repair is completed, the rotating lifting shaft 80 drives the seed crystal holder 70 to rise rapidly, and the temperature continues to rise. As the seed crystal 71 (rotating lifting shaft 80) rises, the transmission device drives the flow guiding device 40 to close slowly, and at the same time, it drives the cover 61 to close slowly. (Reference) Figure 2 As shown, when the seed crystal 71 (rotating lifting shaft 80) rises to the preset position, the guiding device 40 and the cover 61 are completely closed. At this time, the silicon carbide crystal enters the second crystal growth stage. When the temperature inside the outer crucible 30 reaches a certain temperature, the silicon carbide powder sublimates into silicon carbide gas, rises upward, enters the growth space through the guiding device 40, and is deposited on the silicon carbide crystal. In this embodiment, the silicon carbide crystal is first lowered into the inner crucible 62 by the rotating lifting shaft 80 to grow crystals using the Czochralski method, eliminating microtube and dislocation defects. Then, it is lifted to the preset position by the rotating lifting shaft 80 and grown using the vapor phase method, thereby improving the quality of the silicon carbide crystal.
[0031] Furthermore, during the heating process, both the inner crucible 62 and the outer crucible 30 generate heat, resulting in more uniform heating of the silicon carbide powder 31. Simultaneously, this leads to a more uniform radial temperature gradient in the crystal, which is beneficial for improving the growth quality of the silicon carbide crystal. Meanwhile, the inner crucible 62 primarily contains silicon and carbon powder. In the second crystal growth stage, i.e., the vapor phase crystal growth stage, the silicon and carbon powder continuously react to generate SiC. The SiC decomposes upon heating to generate Si2C, SiC2, and Si gas. This rising gas mixes with the sublimated silicon carbide gas from the surrounding silicon carbide powder 31, increasing the silicon vapor content in the mixed gas. Excess silicon vapor can react with carbon particles in the air, thereby reducing the carbon content in the gas and thus reducing impurities such as carbon inclusions, improving crystal quality. The mixed gas passes through the closed porous plate 421, which homogenizes the airflow, further improving the crystal growth quality.
[0032] In some embodiments, the flow guiding device 40 includes an annular flow guiding platform 41 and a flow guiding plate 42. The annular flow guiding platform 41 is connected to the inner wall of the outer crucible 30. A flow guiding hole 44 is defined in the middle of the annular flow guiding platform 41, and the seed crystal holder 70 can pass through the flow guiding hole 44 as the rotating lifting shaft 80 rises and falls. The flow guiding plate 42 is connected to the annular flow guiding platform 41 through a first rotating shaft 43. The first rotating shaft 43 is connected to the connecting part of the rotating lifting shaft 80 through a transmission device. As the rotating lifting shaft 80 rises, the first rotating shaft 43 can drive the flow guiding plate 42 to rotate under the transmission action of the transmission device to block the flow guiding hole 44, thereby closing the flow guiding device 40.
[0033] Specifically, in this embodiment, the rotating lifting device rises and drives the transmission device to move. The transmission device drives the first rotating shaft 43 to rotate and drives the guide plate 42 to rotate, thereby blocking the guide hole 44. When the guide plate 42 does not block the guide hole 44, the guide device 40 is in the open state. When the guide plate 42 blocks the guide hole 44, the guide device 40 is in the closed state.
[0034] refer to Figure 2As shown, in some embodiments, the flow guide plate 42 of the present invention is composed of four 1 / 4 circular perforated plates 421. Each perforated plate 421 is connected to the upper surface of the annular flow guide stage 41 via a first rotating shaft 43. The first rotating shaft 43 is connected to the rotating lifting shaft 80 via a transmission device. When the rotating lifting shaft 80 rises to a preset position, the transmission device drives the perforated plate 421 to rotate and close into the flow guide plate 42 via the first rotating shaft 43, thus blocking the flow guide hole 44 and closing the flow guide device 40. The inner diameter of the outer crucible 30 is 2.1 to 2.2 times the radius of the flow guide plate 42, ensuring that the opening of the perforated plate 421 does not obstruct the descent or ascent of the seed crystal 71, while facilitating the rotation and closure of the perforated plate 421. Specifically, silicon carbide gas enters the growth space through the flow guide plate 42. Since the flow guide plate 42 is composed of perforated plates 421, it has the function of homogenizing the gas, which is beneficial to improving the crystal quality.
[0035] refer to Figure 4 As shown, in some embodiments, the cover 61 of the present invention is a double-door structure composed of two cover plates 611, each cover plate 611 being connected to the side wall of the melting chamber 60 via a hinge; the inner crucible 62 is fixed to the bottom wall inside the melting chamber 60 via a telescopic support frame 50, and the inner crucible 62 descends into the melting chamber 60 as the rotating lifting shaft 80 rises under the drive of the transmission device.
[0036] Specifically, when the rotating lifting shaft 80 is in the initial position, the inner crucible 62 is supported on the upper part of the inner side of the melting chamber 60 by the telescopic support frame, that is, the initial position of the inner crucible 62. When the inner crucible 62 is in the initial position, the two door panels of the cover 61 open to both sides under the force of the inner crucible 62 rising and rest against the side wall of the inner crucible 62. At this time, the cover 61 is in the open state. When the rotating lifting shaft 80 rises, the downward force applied by the transmission device to the inner crucible 62 is greater than the supporting force of the telescopic support frame 50. Under the force of the transmission device, the inner crucible 62 moves downward. When the rotating lifting shaft 80 rises to the preset position, the inner crucible 62 descends to the preset position inside the melting chamber 60. At this time, the two door panels lose the obstruction of the side wall of the inner crucible 62 and, under the action of gravity and hinges, close to the top of the melting chamber 60, thereby shielding the melting chamber 60 and preventing some gas in the melting chamber 60 from entering the growth space, thus avoiding any impact on the quality of the crystal.
[0037] refer to Figure 1 and Figure 2As shown, in some embodiments, the transmission device of the present invention includes a first traction line 921 and a second traction line 931. One end of each first traction line 921 is connected to a connecting component, and the other end passes through the crucible cover 20 and the side wall and bottom wall of the outer crucible 30, and is fixed to the bottom of the inner crucible 62. The first traction line 921 pulls the inner crucible 62 down as the rotating lifting shaft 80 rises, and each first traction line 921 is evenly distributed in the circumferential direction. Specifically, since the length of each first traction line 921 is fixed, when the rotating lifting shaft 80 rises, one end of the first traction line 921 rises accordingly, and the other end of the first traction line 921 pulls the inner crucible 62 down. When the rotating lifting shaft 80 rises to a preset position, the inner crucible 62 completely descends into the melting chamber 60, and the cover 61 closes at the same time.
[0038] Each second traction wire 931 has one end connected to the connecting component, and the other end passes sequentially through the crucible cover 20, the side wall of the outer crucible 30, and the side wall of the annular guide platform 41, winding around the lower part of the first rotating shaft 43. As the rotating lifting shaft 80 rises, the second traction wire 931 drives the perforated plate 421 to rotate and close into the guide plate 42 via the first rotating shaft 43. In this embodiment, there are four second traction wires 931, the same number as the first rotating shaft 43, and the second traction wires 931 are evenly distributed in the circumferential direction. Specifically, the length of the second traction wire 931 in this embodiment is also fixed. One end is wound around the first rotating shaft 43, and the other end is connected to the connecting component of the rotating lifting shaft 80. When the rotating lifting shaft 80 rises, the second traction wire 931 drives the perforated plate 421 to rotate inward and slowly close through the first rotating shaft 43. When the rotating lifting shaft 80 rises to the preset position, the perforated plate 421 is completely closed together to form the guide plate 42, which blocks the guide hole 44.
[0039] In this embodiment, the only power source controlling the movement of the inner crucible 62, the cover 61, and the perforated plate 421 is the rising of the rotating lifting shaft 80. The rising of the rotating lifting shaft 80 pulls the traction line upward, thereby achieving the purpose of lowering the inner crucible 62, closing the cover 61, and rotating and closing the perforated plate 421. This will not interfere with the crystal growth environment inside the outer crucible 30, and therefore will not affect the crystal growth quality, which is conducive to improving the crystal quality.
[0040] Further, refer to Figure 1 and Figure 2As shown, in some embodiments, the transmission device of the present invention further includes a traction wire transmission channel, which mainly consists of a first traction wire transmission channel 91, a second traction wire transmission channel 92, and a third traction wire transmission channel 93. The first traction wire transmission channel 91 is confined within the crucible cover 20, the second traction wire transmission channel 92 is confined within the wall of the outer crucible 30, and the third traction wire transmission channel 93 is confined within the side wall of the annular guide platform 41 in the radial direction. One end of the first traction wire transmission channel 91 is connected to the shaft hole of the rotating lifting shaft 80, and the other end is connected to one end of the second traction wire transmission channel 92. The other end of the second traction wire transmission channel 92 is connected to the bottom of the melting chamber 60. One end of the third traction wire transmission channel 93 is connected to the shaft hole of the first rotating shaft 43, and the other end is connected to the second traction wire transmission channel 92. One end of the first traction wire 921 is connected to a connecting component, and the other end passes through the first transmission channel 91 and the second transmission channel 92 in sequence and is connected to the bottom of the inner crucible 62. One end of the second traction wire 931 is connected to the connecting component, and the other end passes through the first transmission channel 91, the second transmission channel 92, and the third transmission channel 93 in sequence and is wound around the first rotating shaft 43. The number of traction wire transmission channels is the same as that of the first rotating shafts 43, and they are evenly distributed in the circumferential direction on the outer crucible 30 wall and inside the crucible cover 20. The vertical cross-section of the traction wire channel is "E" shaped. Each shaft hole of the first rotating shaft 43 is connected to a corresponding traction wire transmission channel. The shaft hole of the first rotating shaft 43 is connected to the third traction wire transmission channel 93 of the transmission channel.
[0041] Specifically, the first traction wire transmission channel 91 is opened along the side and top walls of the crucible cover 20, the second traction wire transmission channel 92 is opened along the side and bottom walls of the outer crucible 30, and the third traction wire transmission channel 93 is opened along the side wall of the annular guide platform 41 below the perforated plate 421. The first traction wire transmission channel 91 is connected to the second traction wire transmission channel 92, and the third traction wire transmission channel 93 is connected to the second traction wire transmission channel 92. The first traction wire transmission channel 91 is connected to the shaft hole of the rotating lifting shaft 80, and the second traction wire transmission channel 92 is connected to the bottom of the melting chamber 60. The traction wire transmission channels are evenly distributed circumferentially on the wall of the outer crucible 30 and inside the crucible cover 20. In this embodiment, the traction wire transmission channels are opened on the wall of the outer crucible 30 and inside the crucible cover 20. The traction wire passes through the traction wire transmission channels and connects to the bottom of the inner crucible 62 and the first rotating shaft 43, which effectively reduces the friction during the traction wire transmission process, extends the service life of the traction wire, and makes the transmission smoother. Furthermore, to make the transmission smoother, pulleys can be installed at the corners of the traction line transmission channel, and the tension of the traction line in the traction line transmission channel is on the pulleys at the corners.
[0042] In some embodiments, the connecting component of the present invention is a connecting ring 81 or a bearing (not shown in the figure); an annular groove is provided on the side wall of the rotary lifting shaft 80, and the connecting ring 81 or bearing is sleeved on the rotary lifting shaft 80 and located within the annular groove. The outer diameter of the connecting ring 81 or bearing is not greater than the outer diameter of the rotary lifting shaft 80. When the connecting component is a connecting ring 81, the connecting ring 81 and the rotary lifting shaft 80 are clearance-fitted, and the contact surfaces of the connecting ring 81 and the rotary lifting shaft 80 are both polished surfaces. The transmission device is fixedly connected to the connecting ring 81. When the connecting component is a bearing, the inner ring of the bearing is interference-fitted with the rotary lifting shaft 80, and the transmission device is fixedly connected to the outer ring of the bearing. Since the connecting ring 81 and the rotary lifting shaft 80 are clearance-fitted, and the contact surfaces of the connecting ring 81 and the rotary lifting shaft 80 are both polished surfaces, when the rotary lifting shaft 80 rotates, the connecting ring 81 will not rotate with it, and the traction line will not rotate and wrap around the rotary lifting shaft 80.
[0043] Based on the above embodiments, the present invention provides a method for preparing high-quality silicon carbide crystals, specifically including the following steps: 1) Loading: Si powder and C powder are placed in the inner crucible 62 according to the preset ratio. For example, the preset ratio is: molar ratio of Si:C = 1:1.5. Under this ratio, the grown crystal is more flat. Pure SiC powder is placed in the outer crucible 30, and the seed crystal 71 is bonded to the seed crystal holder 70. 2) Adjust the above equipment to its initial state: Both the flow guiding device 40 and the cover 61 are in the open state, that is, the perforated plate 421 is on the annular flow guiding platform 41 outside the flow guiding hole 44; The inner crucible 62 is raised above the melting chamber 60 under the support of the telescopic support frame 50. At this time, the two door panels of the cover 61 rest against the side wall of the inner crucible 62 respectively. The rotating lifting shaft 80 drives the seed crystal 71 down into the inner crucible 62.
[0044] 3) Start the equipment and begin crystal growth, which includes the following two stages: 3.1) First Crystal Growth Stage: At the start of the first crystal growth stage, the temperature is raised to 1500-1700℃, preferably 1550℃. At this time, the inside of the inner crucible 62 is in a molten state, and the silicon carbide seed crystal 71 is grown for 10 hours using the Czochralski method. During the 10 hours, the rotating lifting shaft 80 pulls the seed crystal 71 upward at a speed of 0.05 mm / h. During the upward pulling of the seed crystal 71 (during the first crystal growth stage), the inner crucible 62 is pulled down into the melting chamber 60 by the first traction line 921. The two door plates of the cover 61 move down under the action of gravity. At the same time, the first rotating shaft 43 is pulled and rotated by the second traction line 931, causing the porous plate 421 to rotate inward. When the seed crystal 71 rises to the top of the outer crucible 30 (the preset position of the seed crystal 71), the inner crucible 62 completely descends into the melting chamber 60. At this time, the cover 61 is completely closed, and the porous plate 421 is closed. The first crystal growth stage ends, and the repaired silicon carbide crystal is obtained, and the second crystal growth stage begins. 3.2) The crystal growth time in the second crystal growth stage is 100h, the crystal growth temperature is controlled at 2200-2300℃, the preferred temperature is 2240℃, and the crystal growth pressure is controlled at 6mbar. At the same time, the silicon carbide powder in the outer crucible 30 sublimates into silicon carbide gas, rises upward, and enters the growth space through the guide device 40. The silicon carbide crystal obtained in step 3.1 is grown by gas phase method.
[0045] 4) Crystal growth is complete, and high-quality silicon carbide crystals are obtained.
[0046] Example 3 This embodiment is largely the same as Embodiment 2, except that the connecting components, transmission device, inner crucible 62, and cover 61 structures and driving methods are different in this embodiment. The specific differences are as follows: refer to Figure 5 , Figure 6 and Figure 7 As shown, in some embodiments, the inner crucible 62 of the present invention is fixedly installed on the upper part of the inner side of the melting chamber 60, and the cover 61 is composed of four 1 / 4 circle cover plates 611. Each cover plate 611 is connected to the top of the side wall of the melting chamber 60 through a second rotating shaft. Under the action of the transmission device, the second rotating shaft drives the cover plate 611 to rotate inward as the rotating lifting shaft 80 rises, thereby controlling the closing of the cover 61.
[0047] In some embodiments, the connecting component of the present invention is a rack 95, which is disposed on the outer wall of the rotating lifting shaft 80. The transmission device includes a traction shaft and a gear. The traction shaft includes a first traction shaft 971, a second traction shaft 972, a third traction shaft 973, a fourth traction shaft 974, and a fifth traction shaft 975. One end of the first traction shaft 971 meshes with the rack 95 via a gear. The other end of the first traction shaft 971 is connected to one end of the third traction shaft 973 via the second traction shaft. The other end of the third traction shaft 973 is connected to the first rotating shaft. One end of the third traction shaft 973 is connected to... One end of the fourth traction shaft 974 is connected to one end of the fifth traction shaft 975, and the other end of the fifth traction shaft 975 is connected to the second rotating shaft. The first traction shaft 971 and the second traction shaft 972, the second traction shaft 972 and the third traction shaft 973, the third traction shaft 973 and the first rotating shaft 43, the third traction shaft 973 and the fourth traction shaft 974, the fourth traction shaft 974 and the fifth traction shaft 975, and the fifth traction shaft 975 and the second rotating shaft are all connected by bevel gear pairs 98. There are a total of 4 traction shafts, which are evenly spaced in the circumferential direction.
[0048] Furthermore, to avoid frictional resistance between the traction shaft and the crucible cover 20, the side wall of the outer crucible 30, and the side wall of the annular guide platform 41, and to extend the service life of the traction shaft, the present invention also includes a traction shaft transmission channel. The traction shaft is installed in the traction shaft transmission channel via a fixing ring 94, with a clearance fit between the traction shaft and the fixing ring 94. The traction shaft transmission channel includes a first traction shaft transmission channel 961, a second traction shaft transmission channel 962, and a third traction shaft transmission channel 963. The first traction shaft transmission channel 961 is confined within the crucible cover 20, the second traction shaft transmission channel 962 is confined within the side wall of the outer crucible 30, and the third traction shaft transmission channel 963 is confined within the side wall of the annular guide platform 41. One end of the first traction shaft transmission channel 961 is connected to the rotating lifting shaft 80. One end of the first traction shaft 971 is connected to the shaft hole of the first rotating shaft 43, and the other end is connected to one end of the second traction shaft transmission channel 962. One end of the third traction shaft transmission channel 963 is connected to the shaft hole of the first rotating shaft, and the other end is connected to the second traction shaft transmission channel 962. The number of traction shaft transmission channels is the same as that of the first rotating shaft 43, and each shaft hole of the first rotating shaft 43 corresponds to one traction shaft transmission channel. The first traction shaft 971 and the second traction shaft 972 are respectively placed in the first traction shaft transmission channel and the second traction shaft transmission channel 962. The third traction shaft 973 and the fourth traction shaft 974 are arranged vertically in the second traction shaft transmission channel 962. Each first rotating shaft 43 corresponds to one traction shaft transmission channel. There are a total of four traction shaft transmission channels, which are evenly spaced in the circumferential direction.
[0049] Specifically, the number of traction shaft drive channels is the same as the number of first rotating shafts 43. The traction shaft drive channels are evenly distributed circumferentially on the outer crucible 30 wall and inside the crucible cover 20. Each first rotating shaft 43 corresponds to one traction shaft drive channel, and the third traction shaft drive channel 963 of each traction shaft drive channel is connected to the shaft hole of its nearest first rotating shaft 43. The traction shaft is installed in the traction shaft drive channel through a fixing ring 94. Both ends of each traction shaft and the lower part of the first rotating shaft 43 are provided with a sawtooth structure. The traction shafts are connected to each other and to the traction shafts and to the first rotating shaft 43 and the second rotating shaft through bevel gear pairs 98. The first traction shaft 971 meshes with a rack 95 through a gear. When the rotating lifting shaft 80 rises, the rack 95 on its surface drives the gear to rotate, which in turn drives the first traction shaft 971 to rotate. The first traction shaft 971 then drives the second traction shaft 972 to rotate, which in turn drives the third traction shaft 973 and the fourth traction shaft 974 to rotate. The third traction shaft 973 drives the first rotating shaft 43 to rotate, which in turn drives the perforated plate 421 to rotate inward. At the same time, the fourth traction shaft 974 drives the fifth traction shaft 975 to rotate, which in turn drives the cover plate 611 to rotate inward via the second rotating shaft. When the rotating lifting shaft 80, carrying the seed crystal 71, rises to the preset position, the perforated plate 421 completely closes to form the guide plate 42, thereby closing the guide device 40. Simultaneously, the cover plate 611 closes to block the melting chamber 60. At this point, the first crystal growth stage ends, and the second crystal growth stage begins. In this embodiment, the traction shaft is driven to rotate by the meshing transmission of the bevel gear pair 98, which in turn drives the first rotating shaft 43 and the second rotating shaft to rotate and cause the porous plate 421 and the cover plate 611 to rotate inward and close. The driving method is simple and convenient, and no impurities will be generated to enter the growth space. Therefore, it will not affect the quality of the crystal.
[0050] Based on the equipment of this embodiment, the silicon carbide crystal growth method of this embodiment is as follows: 1) Loading: Si powder and C powder are placed in the inner crucible 62 according to the preset ratio. For example, the preset ratio is Si:C = 1:1.2-1:1.5, and the preferred ratio is Si:C = 1:1.3. Under this ratio, the grown crystal is more flat. Pure SiC powder is placed in the outer crucible 30, and the seed crystal 71 is bonded to the seed crystal holder 70. 2) Adjust the above equipment to its initial state: Both the flow guiding device 40 and the cover 61 are in the open state, that is, the perforated plate 421 is on the annular flow guiding platform 41 outside the flow guiding hole 44; the rotating lifting shaft 80 drives the seed crystal 71 to descend into the inner crucible 62.
[0051] 3) Start the equipment and begin crystal growth, which includes the following two stages: 3.1) First crystal growth stage: At the start of crystal growth, the temperature is raised to 1500-1700℃, preferably 1600℃. At this time, the inside of the inner crucible 62 is in a molten state. The silicon carbide seed crystal 71 is grown using the Czochralski method for 8-10 hours, preferably 10 hours. During the 8-10 hours, the rotating lifting shaft 80 pulls the seed crystal 71 upward at a speed of 0.04-0.06 mm / h, preferably 0.04.5 mm / h. During the upward pulling of the seed crystal 71 (during the first crystal growth stage), the gear rotates as the rack 95 on the outer surface of the rotating lifting shaft rises, and the gear in turn drives the first traction shaft 971 to rotate. Under the action of the bevel gear pair 98, the second traction shaft 972, the third traction shaft 973, the fourth traction shaft 974 and the fifth traction shaft 975 rotate accordingly. The third traction shaft 973 drives the perforated plate 421 to slowly rotate inward and close through the first rotating shaft 43. At the same time, the fifth traction shaft 975 drives the cover plate 611 to slowly rotate inward and close through the second rotating shaft. When the seed crystal 71 rises to the top of the outer crucible 30 (the preset position of the seed crystal 71), the inner crucible 62 completely descends into the interior of the melting chamber 60. At this time, the cover 61 is completely closed, and the perforated plate 421 is completely closed. The first crystal growth stage ends, and the repaired silicon carbide crystal is obtained. The second crystal growth stage begins. 3.2) The crystal growth time in the second crystal growth stage is 90-110h, preferably 95h. The crystal growth temperature is controlled at 2200-2300℃, preferably 2250℃. The crystal growth pressure is controlled at 3-6mbar, preferably 5mbar. At the same time, the silicon carbide powder in the outer crucible 30 sublimates into silicon carbide gas, rises upward, and enters the growth space through the porous plate 421. The silicon carbide crystals obtained in step 3.1 are grown using the gas phase method.
[0052] 4) Crystal growth is complete, and high-quality silicon carbide crystals are obtained.
[0053] Other components of the growth method and apparatus for preparing high-quality silicon carbide crystals according to embodiments of the present invention, such as the inner crucible 62, the outer crucible 30, the retractable support frame 50, and the rotary lifting shaft 80, as well as their operation, are known to those skilled in the art and will not be described in detail here.
[0054] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial," "radial," and "circumferential" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.
[0055] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this invention, "a plurality of" means two or more, unless otherwise explicitly specified.
[0056] In this invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection, an electrical connection, or a communication connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.
[0057] In this invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can mean that the first feature is in direct contact with the second feature, or that the first feature is in indirect contact with the second feature through an intermediate medium. Furthermore, "above," "over," and "on top" of the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.
[0058] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0059] Although embodiments of the invention have been shown and described, those skilled in the art will understand that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the claims and their equivalents.
Claims
1. A method for growing high-quality silicon carbide crystals, characterized in that, include 1) First crystal growth stage: The silicon carbide seed crystal is immersed in the silicon carbide melt and the silicon carbide seed crystal is grown by the Czochralski method; 2) Second crystal growth stage: The silicon carbide seed crystal obtained in step 1) is grown using the vapor phase method.
2. An apparatus for implementing the growth method for preparing high-quality silicon carbide crystals as described in claim 1, characterized in that, include An outer crucible, the top of which is sealed with a crucible lid, defines a first space; A melting chamber is disposed on the inner bottom wall of the outer crucible, and the upper part of the melting chamber has an opening; A cover body, the cover body being mounted on top of the melting chamber; An inner crucible, which is installed within the melting chamber; A flow guiding device, which is connected to the inner wall of the outer crucible; A rotating lifting shaft, the top end of which is located outside the outer crucible and connected to an external rotating lifting device, and the bottom end of which is located inside the outer crucible, and the rotating lifting shaft is coaxially arranged with the inner crucible; Seed crystal holder, wherein the seed crystal holder is installed at the bottom of the rotating lifting shaft and a seed crystal is installed on its lower surface; The transmission device is connected to the rotating lifting shaft via a connecting component. The transmission device controls the closing of the cover as the rotating lifting shaft rises, and also controls the closing of the flow guiding device as the rotating lifting shaft rises. After the flow guiding device closes, it divides the first space into a growth space and a raw material space. The flow guiding device includes: An annular flow guide platform is connected to the inner wall of the outer crucible. A flow guide hole is defined in the middle of the annular flow guide platform, and the seed crystal holder can pass through the flow guide hole as the rotating lifting shaft moves up and down. A guide plate is connected to the annular guide platform via a first rotating shaft. The first rotating shaft is connected to the connecting component of the rotating lifting shaft via the transmission device. As the rotating lifting shaft rises, the first rotating shaft can drive the guide plate to rotate under the action of the transmission device to block the guide hole and close the guide device. The guide plate is composed of four 1 / 4 circle perforated plates.
3. The apparatus for the growth method of preparing high-quality silicon carbide crystals according to claim 2, characterized in that, Each of the perforated plates is connected to the annular guide plate via a first rotating shaft. The first rotating shaft is connected to the rotating lifting shaft via the transmission device. When the rotating lifting shaft rises to a preset position, the transmission device drives the perforated plate to rotate and close into the guide plate via the first rotating shaft, thereby blocking the guide holes and closing the guide device.
4. The apparatus for the growth method of preparing high-quality silicon carbide crystals according to claim 3, characterized in that, The cover is a double-door structure consisting of two cover plates, each of which is connected to the side wall of the melting chamber via hinges; the inner crucible is fixed to the bottom wall inside the melting chamber by a telescopic support frame, and the inner crucible descends into the melting chamber as the rotating lifting shaft rises, driven by the transmission device.
5. The apparatus for the growth method of preparing high-quality silicon carbide crystals according to claim 4, characterized in that, The transmission device includes The first traction line, one end of each first traction line is connected to the connecting component, and the other end passes through the crucible cover and the side wall and bottom wall of the outer crucible in sequence and is fixed to the bottom of the inner crucible. The first traction line pulls the inner crucible down as the rotating lifting shaft rises. The second traction wires are connected at one end to the connecting component, and at the other end, they pass through the crucible cover, the outer crucible sidewall, and the annular guide platform sidewall in sequence and are wound in the same direction around the lower part of the first rotating shaft. As the rotating lifting shaft rises, the second traction wires drive the perforated plate to rotate and close into the guide plate through the first rotating shaft. The first traction line and the second traction line are each provided with four lines, and they are evenly spaced in the circumferential direction.
6. The apparatus for the growth method of preparing high-quality silicon carbide crystals according to claim 5, characterized in that, It also includes traction wire drive channels, which are mainly composed of a first traction wire drive channel, a second traction wire drive channel, and a third traction wire drive channel. The first traction wire drive channel is confined within the crucible lid, the second traction wire drive channel is confined within the outer crucible wall, and the third traction wire drive channel is confined within the side wall of the annular guide platform. One end of the first traction wire drive channel is connected to the shaft hole of the rotating lifting shaft, and the other end is connected to one end of the second traction wire drive channel. The other end of the second traction wire drive channel is connected to the bottom of the melting chamber. One end of the third traction wire drive channel is connected to the shaft hole of the first rotating shaft, and the other end is connected to the second traction wire drive channel. A total of four traction wire drive channels are provided, evenly spaced in the circumferential direction, with each shaft hole of the first rotating shaft corresponding to one traction wire drive channel. One end of the first traction wire is connected to the bottom of the inner crucible, and the other end passes through the second traction wire transmission channel and the first traction wire transmission channel in sequence and is connected to the connecting component; one end of the second traction wire is wound around the first rotating shaft, and the other end passes through the third traction wire transmission channel, the second traction wire transmission channel and the first traction wire transmission channel in sequence and is connected to the connecting component.
7. The apparatus for the growth method of preparing high-quality silicon carbide crystals according to claim 5 or 6, characterized in that, The connecting component is a connecting ring or a bearing. The side wall of the rotating lifting shaft is provided with an annular groove. The connecting ring or bearing is sleeved on the rotating lifting shaft and placed in the annular groove. The outer diameter of the connecting ring or bearing is not greater than the outer diameter of the rotating lifting shaft. When the connecting component is a connecting ring, the connecting ring and the rotating lifting shaft are in clearance fit, and the contact surfaces of the connecting ring and the rotating lifting shaft are both polished surfaces. The transmission device is fixedly connected to the connecting ring. When the connecting component is a bearing, the inner ring of the bearing is interference-fitted with the rotating lifting shaft, and the transmission device is fixedly connected to the outer ring of the bearing.
8. The apparatus for the growth method of preparing high-quality silicon carbide crystals according to claim 2, characterized in that, The inner crucible is fixedly installed on the upper side of the melting chamber. The cover is composed of four quarter-circle cover plates. Each cover plate is connected to the top of the side wall of the melting chamber through a second rotating shaft. Under the action of the transmission device, the second rotating shaft drives the cover plate to rotate inward as the rotating lifting shaft rises, thereby controlling the closing of the cover.
9. The apparatus for the growth method of preparing high-quality silicon carbide crystals according to claim 8, characterized in that, The connecting part is a rack, which is disposed on the outer wall of the rotating lifting shaft. The transmission device includes a traction shaft and gears. The traction shaft includes a first traction shaft, a second traction shaft, a third traction shaft, a fourth traction shaft, and a fifth traction shaft. One end of the first traction shaft meshes with the rack via a gear. The other end of the first traction shaft is connected to one end of the third traction shaft via the second traction shaft. The other end of the third traction shaft is connected to a first rotating shaft. One end of the third traction shaft is connected to one end of the fifth traction shaft via the fourth traction shaft. The other end of the fifth traction shaft is connected to the second rotating shaft. The first traction shaft and the second traction shaft, the second traction shaft and the third traction shaft, the third traction shaft and the first rotating shaft, the third traction shaft and the fourth traction shaft, the fourth traction shaft and the fifth traction shaft, and the fifth traction shaft and the second rotating shaft are all connected by bevel gear pairs. There are a total of 4 traction shafts, which are evenly spaced in the circumferential direction.
10. The apparatus for the growth method of preparing high-quality silicon carbide crystals according to claim 9, characterized in that, It also includes a traction shaft drive channel, in which the traction shaft is installed by a fixing ring, and the traction shaft and the fixing ring are clearance-fitted. The traction shaft drive channel includes a first traction shaft drive channel, a second traction shaft drive channel, and a third traction shaft drive channel. The first traction shaft drive channel is confined within the crucible cover, the second traction shaft drive channel is confined within the side wall of the outer crucible, and the third traction shaft drive channel is confined within the side wall of the annular guide platform. One end of the first traction shaft drive channel communicates with the shaft hole of the rotating lifting shaft, and the other end communicates with one end of the second traction shaft drive channel. One end of the third traction shaft drive channel communicates with the shaft hole of the first rotating shaft, and the other end communicates with the second traction shaft drive channel. The number of traction shaft drive channels is the same as the number of first rotating shafts, and each shaft hole of the first rotating shaft corresponds to one traction shaft drive channel. The first traction shaft and the second traction shaft are respectively placed in the first traction shaft drive channel and the second traction shaft drive channel, and the third traction shaft and the fourth traction shaft are arranged vertically in the second traction shaft drive channel. Each first rotating shaft corresponds to one traction shaft drive channel. There are four traction shaft drive channels, which are evenly spaced in the circumferential direction.
Citation Information
Patent Citations
Silicon carbide crystal growth device and growth method thereof