A method for preparing chitin / chitosan material composite with natural calcium carbonate

Through deprotein and oxidative decolorization treatment, combined with deacetylation treatment of alkali aqueous solution, chitin/chitosan-calcium carbonate composite materials without additional addition of inorganic calcium sources, solving the low activity and high cost of inorganic calcium sources in traditional methods Problem, high-strength, low-cost and environmentally friendly composite materials production has been achieved.

CN116554557BActive Publication Date: 2024-11-22WUHAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210114153.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-01-30
Publication Date
2024-11-22
Estimated Expiration
2042-01-30

AI Technical Summary

Technical Problem

Among the existing synthetic calcium carbonate-containing composite materials, the traditional inorganic calcium source has low activity and poor solubility, making it difficult to form effective interaction with the organic template, resulting in the structural morphology of the composite material being difficult to control, poor uniformity, and additional inorganic Calcium sources will increase costs, destroy the structure of natural calcium carbonate, and cause environmental pollution.

Method used

After deprotein treatment, the H2O2 aqueous solution was used for oxidation and decolorization, and then deacetylation was performed in the alkali aqueous solution to prepare chitin/chitosan-calcium carbonate composite material without additional inorganic calcium source, and casting film was used. Gel forming or aerogel preparation method retains the structural form of natural calcium carbonate.

Benefits of technology

It realizes high strength, low cost and environmentally friendly production of chitin/chitosan-calcium carbonate materials, and retains the original structural form, is suitable for industrial production, and has excellent mechanical properties and biocompatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116554557B_ABST
    Figure CN116554557B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of natural polymers and polymer materials, and in particular to a method for preparing a chitin / chitosan material of a composite natural calcium carbonate, wherein a raw material containing natural calcium carbonate and chitin / chitosan is subjected to deproteinization treatment, and then subjected to oxidative decolorization treatment with a 1-5wt% H2O2 aqueous solution, and then subjected to deacetylation reaction, and a raw material containing natural calcium carbonate and chitin / chitosan of different deacetylation degrees is obtained after washing. Chitin / chitosan-natural calcium carbonate raw material is dissolved under alkaline conditions to prepare a chitin material of composite natural calcium carbonate or a chitosan material of composite natural calcium carbonate. The present invention is different from a complex formed by general chitin / chitosan composite inorganic salts, and the obtained chitin / chitosan-natural calcium carbonate complex is a natural composite material, which has a wide range of application prospects in the fields of functional materials such as environmentally friendly materials and biomimetic materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of natural polymers and polymer materials, and in particular to a method for preparing a chitin / chitosan material composited with natural calcium carbonate. Background Art

[0002] Biomineralization is the process of generating inorganic minerals under the participation and regulation of organisms. It is a biochemical and physical phenomenon that is widely present in nature. Since the formation and growth of inorganic phases are strictly controlled by organic matter secreted by organisms, the biomineralization process can generally form natural composite materials with orderly arrangement, excellent structure and performance. Calcium carbonate, as a major biomineral, is widely present in crustaceans such as shrimps and crabs, as well as in the shells of mollusks. At the same time, the main components of various biological organs such as bones and shells are calcium-based biofilms. Therefore, calcium carbonate has become a research hotspot for researchers to design new organic-inorganic composite materials due to its abundant resources and excellent performance.

[0003] Chitosan is the second largest natural polymer in nature after cellulose. It is widely found in arthropods (such as shrimps and crabs), mollusks (such as squids and cuttlefish), annelids, coelenterates, fungi and algae. In biological tissues, chitosan usually forms protective and functional tissues required by organisms in the form of symbiosis or eutectics with minerals, proteins or colloids, and the stacking state of chitosan in different organisms is significantly different. For example, in lobster fore claws and crab shells, chitosan molecules are assembled into 3-20nm nanofibers through hydrogen bonds. These nanofibers are arranged in parallel to form a layered structure, and then stacked with mineral salts to form a unique Bouligand structure. This structure helps to prevent the increase of cracks and defects. Its hardness is enough to resist most external impacts in nature and provide protection for lobsters and crabs (Science 2013, 339, 773-779). It can be seen that the study of the multi-level structure, strength and structure-activity relationship of chitin in biological hard tissues such as lobster fore claws, crab shells, and pearl oysters provides a theoretical structural guidance for the preparation of high-strength organic-inorganic composite materials (Prog. Mater. Sci. 2012, 57, 1492-1704). Using chitin or its derivative chitosan as an organic template, chitosan / chitosan-calcium carbonate composite materials with excellent performance can be obtained.

[0004] At present, artificially synthesized composite materials containing calcium carbonate usually use an external calcium source to obtain calcium carbonate through calcium carbonate deposition or induced crystallization. The main defects of this method are that the traditional inorganic calcium source has low activity and poor solubility, and it is often difficult to produce effective interactions with organic templates such as chitin, chitosan, polyacrylic acid, etc. The resulting composite materials, such as thin film structures, are difficult to control and have poor uniformity. In addition, the additional addition of inorganic calcium sources will increase costs. The main components of shrimp shells and crab shells are calcium carbonate, chitin and protein. The traditional chitin preparation method usually uses acid to remove calcium carbonate, which not only destroys the structure and activity of natural calcium carbonate, but also does not effectively utilize calcium carbonate. In addition, the high additional costs caused by the use of a large amount of acid and the impact of the generated carbon dioxide on the environment are all current problems. Based on this, if the natural calcium carbonate in shrimp shells and crab shells can be retained, and only the protein and pigment in them can be removed, and a suitable solvent can be found to dissolve the chitin or chitosan that is composited with natural calcium carbonate, and the dissolved chitosan / chitosan-calcium carbonate complex solution can be used to prepare materials, it can not only save costs but also retain the original structural morphology of chitin and calcium carbonate, thereby obtaining a composite material with excellent performance. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a chitin / chitosan material composited with natural calcium carbonate, which does not require the addition of an additional inorganic calcium source while retaining the structural morphology of natural calcium carbonate. The prepared chitin / chitosan-calcium carbonate material has high strength, a simple process, low cost, is green and environmentally friendly, and is suitable for industrial production.

[0006] The solution adopted by the present invention to achieve the purpose is: a method for preparing a chitin / chitosan material composite with natural calcium carbonate, comprising the following steps:

[0007] (1) deproteinizing the raw material containing natural calcium carbonate and chitin / chitosan, and then oxidizing and decolorizing it with a 1-5 wt% H2O2 aqueous solution, washing it, and then drying it;

[0008] (2) deacetylation of the product obtained in step (1) with an alkaline aqueous solution of 20 wt % or more at 60-170° C., and obtaining a mixture of composite calcium carbonate chitin with a deacetylation degree of no more than 50% and an alkaline aqueous solution or a mixture of composite calcium carbonate chitosan with a deacetylation degree of more than 50% and an alkaline aqueous solution by controlling the degree of deacetylation, and removing the alkali from the mixture and drying it to obtain composite calcium carbonate chitin or composite calcium carbonate chitosan;

[0009] (3) preparing a chitin-calcium carbonate composite solution or a chitosan-calcium carbonate composite solution with an alkali concentration of 5 wt% to 30 wt%;

[0010] (4) preparing a chitin material composited with natural calcium carbonate or a chitosan material composited with natural calcium carbonate, comprising any one of the following methods: A1, casting the chitin-calcium carbonate composite solution or the chitosan-calcium carbonate composite solution obtained in step (3) into a film, immersing it in a coagulant for coagulation and regeneration to obtain a chitin-calcium carbonate wet film or a chitosan-calcium carbonate wet film, washing away the chemical reagent in the wet film with water, and obtaining a chitin-calcium carbonate film or a chitosan-calcium carbonate film after stretching and drying; A2, adding the chitin-calcium carbonate composite solution or the chitosan-calcium carbonate composite solution obtained in step (3) to the chitin-calcium carbonate composite solution; A cross-linking agent is added to a chitosan-calcium carbonate composite solution and stirred evenly, and the solution is placed in an environment close to the gelation temperature and heated to form a gel, and then immersed in a coagulant below its gelation temperature to regenerate the gel, and the chemical reagents in the gel are removed to obtain a chitin-calcium carbonate hydrogel or a chitosan-calcium carbonate hydrogel; A3, preparing a chitosan-calcium carbonate hydrogel or a chitosan-calcium carbonate hydrogel, replacing the hydrogel with anhydrous ethanol or acetone for several times, and then performing supercritical carbon dioxide drying to remove the liquid to obtain a chitosan-calcium carbonate aerogel or a chitosan-calcium carbonate aerogel.

[0011] In step (1), the deproteinization operation steps are: preparing a sodium hydroxide aqueous solution with a mass fraction of more than 4wt% or a potassium hydroxide aqueous solution with a mass fraction of more than 5.6wt%, soaking the crab shells in the sodium hydroxide or potassium hydroxide aqueous solution at a material-liquid ratio of 1:100 to 1:4 of the raw material containing natural calcium carbonate and chitin / chitosan to the sodium hydroxide aqueous solution or the potassium hydroxide aqueous solution, and soaking at 25°C to 80°C for more than 1h to remove the protein.

[0012] Preferably, in step (1), the raw material containing natural calcium carbonate and chitin / chitosan is crab shell or shrimp shell, the material-liquid ratio of the raw material containing natural calcium carbonate and chitin / chitosan to the H2O2 aqueous solution is 1:10-30, and the temperature of the oxidative decolorization treatment is 40° C. to 100° C. The raw material containing natural calcium carbonate and chitin / chitosan may also be one or more of the shells of other molluscs rich in calcium carbonate.

[0013] Preferably, in step (2), the alkaline aqueous solution is a sodium hydroxide aqueous solution or a potassium hydroxide aqueous solution, and the solid-liquid ratio of the product to the alkaline aqueous solution is 1:10-100.

[0014] When potassium hydroxide aqueous solution is used, the concentration of the aqueous alkali solution is 30 wt % or more, and when sodium hydroxide aqueous solution is used, the concentration of the aqueous alkali solution is 20 wt % or more.

[0015] Preferably, in the step (3), the preparation of a chitosan-calcium carbonate composite solution or a chitosan-calcium carbonate composite solution with an alkali concentration of 5wt% to 30wt% is any one of the following methods: B1, preparing a potassium hydroxide aqueous solution with a concentration of 5wt% to 30wt%, adding a stabilizer, composite calcium carbonate chitosan or composite calcium carbonate chitosan, mixing well, freezing to below freezing point, and then thawing above freezing point to dissolve the composite calcium carbonate chitosan or composite calcium carbonate chitosan to obtain a chitosan-calcium carbonate composite solution or a chitosan-calcium carbonate composite solution; B2, preparing a potassium hydroxide aqueous solution with a concentration of 5wt% to 30wt%, Add a stabilizer, composite calcium carbonate chitin or composite calcium carbonate chitosan, and continuously stir and dissolve at a temperature above freezing point and below 0°C to obtain a chitosan-calcium carbonate composite solution or a chitosan-calcium carbonate composite solution; B3, prepare an aqueous solution of potassium hydroxide or sodium hydroxide with a concentration of 25wt% to 60wt%, add the composite calcium carbonate chitosan or composite calcium carbonate chitosan, place the mixed solution at 0 to 10°C for a period of time, then add ice cubes or ice water to dilute the alkali concentration to 5wt% to 30wt%, stir to dissolve the composite calcium carbonate chitosan or composite calcium carbonate chitosan, and obtain a chitosan-calcium carbonate composite solution or a chitosan-calcium carbonate composite solution.

[0016] In B3, a chitosan-calcium carbonate composite solution is prepared. When potassium hydroxide is used, a potassium hydroxide aqueous solution with a concentration of 35wt% to 60wt% is prepared, and composite calcium carbonate chitosan is added. After the mixed solution is placed at 0 to 10°C for a period of time, ice cubes or ice water are added to dilute the potassium hydroxide concentration to 10wt% to 30wt%, and the composite calcium carbonate chitosan is dissolved after stirring to obtain a chitosan-calcium carbonate composite solution. When sodium hydroxide is used, a sodium hydroxide aqueous solution with a concentration of 25wt% to 50wt% is prepared, and composite calcium carbonate chitosan is added. After the mixed solution is placed at 0 to 10°C for a period of time, ice cubes or ice water are added to dilute the sodium hydroxide concentration to 8wt% to 20wt%, and the composite calcium carbonate chitosan is dissolved after rapid stirring above the freezing point and below 0°C to obtain a chitosan-calcium carbonate composite solution.

[0017] The chitosan-calcium carbonate composite solution is prepared by preparing a potassium hydroxide aqueous solution with a concentration of 20wt% to 60wt%, adding the composite calcium carbonate chitosan, placing the mixed solution at 0 to 10°C for a period of time, adding ice cubes or ice water to dilute the potassium hydroxide concentration to 5wt% to 20wt%, stirring to dissolve the composite calcium carbonate chitosan, and obtaining the chitosan-calcium carbonate composite solution; and by preparing a sodium hydroxide aqueous solution with a concentration of 25wt% to 50wt%, adding the composite calcium carbonate chitosan, placing the mixed solution at 0 to 10°C for a period of time, adding ice cubes or ice water to dilute the sodium hydroxide concentration to 5wt% to 20wt%, stirring rapidly to dissolve the composite calcium carbonate chitosan, and obtaining the chitosan-calcium carbonate composite solution.

[0018] Preferably, the stabilizer is urea, thiourea, polyethylene glycol, and the concentration of the stabilizer in the chitin-calcium carbonate composite solution or the chitosan-calcium carbonate composite solution is 0-20wt%.

[0019] Adding stabilizers such as urea, thiourea, polyethylene glycol, etc. helps the continued dissolution of chitin or chitosan and increases the stability of chitin and chitosan solutions. In the chitin-calcium carbonate composite solution or chitosan-calcium carbonate composite solution, the concentration of the stabilizer is: when urea is used, the concentration is 0-20wt%, when thiourea is used, the concentration is 0-6wt%, and when polyethylene glycol is used, the concentration is 0-10wt%.

[0020] Preferably, in step (3), the concentration of the chitin-calcium carbonate composite solution or the chitosan-calcium carbonate composite solution is 1 wt% to 10 wt%.

[0021] Preferably, in step (4), the coagulant is a mixed liquid of any one or more of water, saline solution, and low-viscosity organic liquid soluble in water.

[0022] Preferably, the salt is a salt containing monovalent cations and anions or divalent cations and anions; the water-soluble low-viscosity organic liquid is at least one of alcohols, ketones, esters, amides, and organic sulfides.

[0023] The salt is potassium salt, sodium salt, magnesium salt, chloride salt, acetate, nitrate, sulfate, carbonate; the alcohol is methanol or ethanol; the ketone is acetone; the ester is ethyl acetate; the amide is dimethylamide or dimethylacetamide; and the organic sulfide is dimethyl sulfoxide.

[0024] Preferably, in step (4), the molar ratio of the crosslinking agent, composite calcium carbonate chitin or composite calcium carbonate chitosan chitosan is 0 to 5:1, and the crosslinking agent is an epoxy compound, a glycidyl ether compound, an acrylate or an aldehyde compound.

[0025] The crosslinking agent is a mixture of one or more of epichlorohydrin, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, bisphenol A diglycidyl ether, polypropylene glycol diglycidyl ether, poly(ethylene glycol) diacrylate, malondialdehyde, and glutaraldehyde.

[0026] Preferably, in step (4), the drafting ratio is 1 to 2.5, and when preparing the chitosan material for composite natural calcium carbonate, the solidification regeneration temperature is (-20) to 50°C, and when preparing the chitosan material for composite natural calcium carbonate, the solidification regeneration temperature is 0-100°C.

[0027] The chitin-calcium carbonate wet film stretching ratio is 1-2, and the chitosan-calcium carbonate wet film stretching ratio is 1-2.5.

[0028] Under the premise of not damaging the mechanical properties, additives such as plasticizers, dyes, light stabilizers, etc. can be contained. These additives can be added before the solution is immersed in the coagulation bath.

[0029] The present invention has the following advantages and beneficial effects:

[0030] (1) The preparation method of the present invention not only greatly saves the cost of raw materials and improves the utilization efficiency of raw materials, but also has greater adjustability in the functionalization of chitin / chitosan-calcium carbonate materials, and has broad application prospects in the fields of bionics, separation and adsorption, industrial papermaking, biomedicine, etc.

[0031] (2) The solvents used in the preparation method of the present invention are alkali, urea or thiourea, and water. Compared with organic solvents such as ionic liquids and deep eutectic solvents, the alkali, urea, etc. used can be recycled, which is low-cost, clean and environmentally friendly, and is conducive to industrial production.

[0032] (3) The chitin / chitosan material of composite natural calcium carbonate prepared by the preparation method of the present invention has excellent mechanical properties, thermal stability and biocompatibility, and can be used in many fields such as food packaging, water treatment, biomedical materials, bionic materials, etc.

[0033] (4) The chitin / chitosan material of composite natural calcium carbonate prepared by the preparation method of the present invention retains the structural morphology of natural calcium carbonate and chitin or chitosan, and the preparation process is simple and low-cost. It can make full use of the advantages of the raw materials themselves without the need to add additional inorganic calcium sources, and has high comprehensive utilization efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a scanning electron microscope image of the chitosan-calcium carbonate film hydrogel prepared in Example 4 of the present invention before drying;

[0035] Figure 2This is a scanning electron microscope image of the cross section of the chitosan-calcium carbonate film hydrogel prepared in Example 4 of the present invention before drying. DETAILED DESCRIPTION

[0036] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.

[0037] Example 1

[0038] The crab shell powder was added to a 4wt% NaOH aqueous solution and soaked at room temperature for 24h to remove protein, and then washed with deionized water. The alkali-treated crab shell powder was soaked in a 1wt% H2O2 solution, pH was adjusted to 9, and the pigment, fatty acid, etc. were removed by heating at 80°C for 90min, and then washed with deionized water and dried. A KOH / urea mixed aqueous solution with a mass fraction of 20wt% and 4wt% of KOH and urea was prepared, cooled to 5°C, and the purified chitosan-calcium carbonate powder was added to the aqueous solution, the mass fraction of the chitosan-calcium carbonate powder was 4wt%, and the chitosan-calcium carbonate powder was quickly stirred and dissolved above the freezing point, and a milky chitosan-calcium carbonate solution was obtained after centrifugal degassing. The chitosan-calcium carbonate solution was cast on a glass plate, solidified in a 60wt% CH3COOK solution at 0°C for 1h to form a milky film, and the residual chemical reagents in the film were removed with deionized water to obtain a chitosan-calcium carbonate wet film, with a tensile strength of 1.4MPa and an elongation at break of 80%. The wet chitosan-calcium carbonate film was fixed on a plexiglass plate and dried at room temperature to obtain a white, foldable chitosan-calcium carbonate film with a tensile strength of 70 MPa and an elongation at break of 10%.

[0039] Example 2

[0040] Add crab shell powder to 4wt% NaOH aqueous solution and soak at room temperature for 24h to remove protein, wash with deionized water, soak alkali-treated crab shell powder in 3wt% H2O2 solution, adjust pH=9, heat at 80℃ for 40min to remove pigment, fatty acid, etc., wash with deionized water and dry. Prepare KOH / urea mixed aqueous solution with mass fractions of KOH and urea of ​​20wt% and 4wt% respectively, cool to 5℃, add purified chitosan-calcium carbonate powder to the aqueous solution, the mass fraction of chitosan-calcium carbonate powder is 3wt%, stir evenly and place in -20℃ refrigerator for 12h, thaw at room temperature, centrifuge and degas to obtain milky chitosan-calcium carbonate solution. The chitosan-calcium carbonate solution was cast on a glass plate, solidified in a 40wt% K2CO3 solution at 0°C for 1h to form a milky white film, and the residual chemical reagents in the film were removed with deionized water to obtain a chitosan-calcium carbonate wet film, which had a tensile strength of 0.8Mpa and an elongation at break of 70%. The chitosan-calcium carbonate wet film was fixed on a plexiglass plate and dried at room temperature to obtain a white, foldable chitosan-calcium carbonate film, which had a tensile strength of 62Mpa and an elongation at break of 9%.

[0041] Example 3

[0042] The crab shell powder was added to a 4wt% NaOH aqueous solution and soaked at room temperature for 24h to remove protein, and then washed with deionized water. The alkali-treated crab shell powder was soaked in a 5wt% H2O2 solution, pH was adjusted to 9, and the pigment, fatty acid, etc. were removed by heating at 80°C for 30min, and then washed with deionized water and dried. A 40wt% KOH aqueous solution was prepared, cooled to 5°C, and the purified chitosan-calcium carbonate powder was added to the aqueous solution. The mass fraction of the chitosan-calcium carbonate powder was 6wt%, and placed at 5°C for 12h. Ice water was added to dilute the KOH concentration to 20wt%, and the solution was quickly stirred and dissolved. After centrifugal degassing, a milky white chitosan-calcium carbonate solution was obtained. The chitosan-calcium carbonate solution was cast on a glass plate, and solidified in a 65wt% CH3COOK solution at 0°C for 2h to form a milky white film. The residual chemical reagents in the film were removed with deionized water to obtain a chitosan-calcium carbonate wet film, which had a tensile strength of 2.2MPa and an elongation at break of 76%. The wet chitosan-calcium carbonate film was fixed on a plexiglass plate and dried at room temperature to obtain a white, foldable chitosan-calcium carbonate film with a tensile strength of 65 MPa and an elongation at break of 8%.

[0043] Example 4

[0044] The crab shell powder is added to a 4wt% NaOH aqueous solution and soaked at room temperature for 24h to remove protein, and then washed with deionized water. The alkali-treated crab shell powder is soaked in a 3wt% H2O2 solution, pH=9 is adjusted, and the pigment, fatty acid, etc. are removed by heating at 80°C for 40min, and then washed with deionized water and dried. A 30wt% KOH aqueous solution is prepared, and the purified chitosan-calcium carbonate raw material is added to the KOH aqueous solution, and heated at 80°C for 1h to obtain a mixed solution of chitosan-calcium carbonate and alkali with a deacetylation degree of about 15%, and then cooled to 0°C and water and urea are added to make the KOH mass fraction in the mixed solution 18wt%, the urea mass fraction 10wt%, and the chitosan-calcium carbonate mass fraction 4wt%, and the mixture is quickly stirred and dissolved above the freezing point, and a milky chitosan-calcium carbonate solution is obtained after centrifugal degassing. The chitosan-calcium carbonate solution was cast on a glass plate and solidified in a 40wt% K2CO3 solution at 5°C for 3h to form a milky white film. The residual chemical reagents in the film were removed with deionized water to obtain a chitosan-calcium carbonate wet film with a tensile strength of 1.2MPa and an elongation at break of 67%. The chitosan-calcium carbonate wet film was fixed on a plexiglass plate and dried at room temperature to obtain a white, foldable chitosan-calcium carbonate film with a tensile strength of 58MPa and an elongation at break of 7%. Figure 1 As shown in FIG. 1 , it is a scanning electron microscope image of the hydrogel of the chitosan-calcium carbonate membrane prepared in this embodiment before drying. It can be seen from the image that the chitosan fiber network has uniform pores. Figure 2 This is a scanning electron microscope image of the cross section of the hydrogel of the chitosan-calcium carbonate film prepared in Example 4 of the present invention before drying. It can be seen from the image that the calcium carbonate is embedded in the fiber network and evenly distributed.

[0045] Example 5

[0046] The crab shell powder is added to a 4wt% NaOH aqueous solution and soaked at room temperature for 24h to remove protein, and then washed with deionized water. The alkali-treated crab shell powder is soaked in a 3wt% H2O2 solution, pH=9 is adjusted, and the pigment, fatty acid, etc. are removed by heating at 80°C for 40min, and then washed with deionized water and dried. A KOH aqueous solution with a mass fraction of 60wt% is prepared, and the purified chitosan-calcium carbonate raw material is added to the KOH aqueous solution, and heated at 60°C for 90min to obtain a mixed solution of chitosan-calcium carbonate and alkali with a deacetylation degree of about 30%, cooled to 0°C, and water and urea are added to make the KOH mass fraction in the mixed solution 18wt%, the urea mass fraction 10wt%, and the chitosan-calcium carbonate mass fraction 8wt%, and the mixture is quickly stirred and dissolved above the freezing point, and a milky chitosan-calcium carbonate solution is obtained after centrifugal degassing. The chitosan-calcium carbonate solution was cast on a glass plate and solidified in an ethanol solution at 0°C for 5 hours to form a milky white film. The residual chemical reagents in the film were removed with deionized water to obtain a chitosan-calcium carbonate wet film, which had a tensile strength of 3.2MPa and an elongation at break of 85%. The chitosan-calcium carbonate wet film was fixed on a plexiglass plate and dried at room temperature to obtain a white, foldable chitosan-calcium carbonate film, which had a tensile strength of 78MPa and an elongation at break of 11%.

[0047] Example 6

[0048] Add crab shell powder to 4wt% NaOH aqueous solution and soak at room temperature for 24h to remove protein, wash with deionized water, soak alkali-treated crab shell powder in 3wt% H2O2 solution, adjust pH=9, heat at 80℃ for 40min to remove pigments, fatty acids, etc., wash with deionized water and dry. Prepare a 40wt% NaOH aqueous solution, cool to 5℃, add purified chitosan-calcium carbonate powder to the aqueous solution, the mass fraction of chitosan-calcium carbonate powder is 5wt%, place at 5℃ for 12h, add ice water to dilute the NaOH concentration to 14wt%, stir quickly to dissolve, and obtain a milky chitosan-calcium carbonate solution after centrifugal degassing. The chitosan solution was poured into a perforated plate mold with a diameter of 10 mm and a height of 10 mm, and then immersed in an ethanol aqueous solution with a water content of 90 wt%. After immersion for 12 hours, the chitosan gel was taken out and washed with deionized water to obtain a chitosan hydrogel with a compressive fracture stress of 4.2 MPa and a fracture strain of 55%.

[0049] Example 7

[0050] The crab shell powder is added to a 4wt% NaOH aqueous solution and soaked at room temperature for 24h to remove protein, and then washed with deionized water. The alkali-treated crab shell powder is soaked in a 3wt% H2O2 solution, pH=9 is adjusted, and the pigment, fatty acid, etc. are removed by heating at 40°C for 90min, and then washed with deionized water and dried. A 30wt% KOH aqueous solution is prepared, and the purified chitosan-calcium carbonate raw material is added to the KOH aqueous solution, and heated at 170°C for 10min to obtain a mixed solution of chitosan-calcium carbonate and alkali with a deacetylation degree of about 15%, and then cooled to 0°C, water and urea are added to make the KOH mass fraction in the mixed solution 18wt%, the urea mass fraction 6wt%, and the chitosan-calcium carbonate mass fraction 6wt%, and the mixture is quickly stirred and dissolved above the freezing point, and a milky chitosan-calcium carbonate solution is obtained after centrifugal degassing. Epichlorohydrin was added in an amount equivalent to 2 times the molar ratio of chitin monomer, stirred, centrifuged for degassing, and poured into a perforated plate mold with a diameter of 10 mm and a height of 10 mm. After thermal molding at 30°C, it was immersed in a KCl aqueous solution with a salt concentration of 20 wt%. After soaking for 1 hour, the chitosan gel was taken out and washed with deionized water to obtain a chitosan hydrogel with a compressive fracture stress of 4.6 MPa and a fracture strain of 88%.

[0051] Example 8

[0052] The crab shell powder is added to a 4wt% NaOH aqueous solution and soaked at room temperature for 24h to remove protein, and then washed with deionized water. The alkali-treated crab shell powder is soaked in a 3wt% H2O2 solution, pH=9 is adjusted, and the pigment, fatty acid, etc. are removed by heating at 100°C for 15min, and then washed with deionized water and dried. A KOH aqueous solution with a mass fraction of 60wt% is prepared, and the purified chitosan-calcium carbonate raw material is added to the KOH aqueous solution, and heated at 50°C for 30min to obtain a mixed solution of chitosan-calcium carbonate and alkali with a deacetylation degree of about 30%, and then cooled to 0°C and water and urea are added to make the KOH mass fraction in the mixed solution 20wt%, the urea mass fraction 4wt%, and the chitosan-calcium carbonate mass fraction 8wt%, and the mixture is quickly stirred and dissolved above the freezing point, and a milky chitosan-calcium carbonate solution is obtained after centrifugal degassing. Add ethylene glycol diglycidyl ether equivalent to 0.8 times the molar ratio of chitin monomer, stir, centrifuge and degas, then pour into a perforated plate mold with a diameter of 10mm and a height of 10mm. After thermal molding at 30°C, soak it in a 50wt% CH3COOK-70wt% ethanol aqueous solution. After soaking for 12 hours, take out the chitosan gel and wash it with deionized water to obtain chitosan hydrogel. Continue to place it in ethanol for replacement to obtain chitosan ethanol gel, which is dried at the critical point of carbon dioxide to prepare chitosan aerogel. The specific surface area was tested by nitrogen adsorption, and the BET specific area of ​​the aerogel was measured to be 430m 2 / g, and the compressive stress of the aerogel was 70MPa when the compressive strain was 80% measured by a universal testing machine, and there was no cracking.

[0053] Example 9

[0054] The crab shell powder is added to a 4wt% NaOH aqueous solution and soaked at room temperature for 24h to remove protein, and then washed with deionized water. The alkali-treated crab shell powder is soaked in a 3wt% H2O2 solution, pH=9 is adjusted, and the pigment, fatty acid, etc. are removed by heating at 80°C for 40min, and then washed with deionized water and dried. A 60wt% KOH aqueous solution is prepared, and the purified chitosan-calcium carbonate raw material is added to the KOH aqueous solution, and heated at 80°C for 30min to obtain a mixed solution of chitosan-calcium carbonate and alkali with a deacetylation degree of about 60%, and water and urea are added after cooling to make the KOH mass fraction in the mixed solution 12wt%, the urea mass fraction 6wt%, and the chitosan-calcium carbonate mass fraction 4wt%, and the mixture is quickly stirred and dissolved at 10°C, and a milky chitosan-calcium carbonate solution is obtained after centrifugal degassing. The chitosan-calcium carbonate solution was cast on a glass plate, solidified in a 65wt% CH3COOK solution at 40°C for 20 minutes to form a milky white film, and the residual chemical reagents in the film were removed with deionized water to obtain a chitosan-calcium carbonate wet film, which had a tensile strength of 0.3MPa and an elongation at break of 160%. The chitosan-calcium carbonate wet film was fixed on a plexiglass plate and dried at room temperature to obtain a white, foldable chitosan-calcium carbonate film, which had a tensile strength of 76MPa and an elongation at break of 12%.

[0055] Example 10

[0056] The crab shell powder is added to a 4wt% NaOH aqueous solution and soaked at room temperature for 24h to remove protein, and then washed with deionized water. The alkali-treated crab shell powder is soaked in a 3wt% H2O2 solution, adjusted to pH=9, heated at 80°C for 40min to remove pigments, fatty acids, etc., washed with deionized water and then dried. A 60wt% KOH aqueous solution is prepared, and the purified chitin-calcium carbonate raw material is added to the KOH aqueous solution, heated at 80°C for 1h to obtain a mixed solution of chitosan-calcium carbonate and alkali with a deacetylation degree of about 80%, and water and urea are added after cooling to make the KOH mass fraction in the mixed solution 14wt%, the urea mass fraction 8wt%, and the chitosan-calcium carbonate mass fraction 6wt%, and it is frozen below the freezing point, and then thawed and dissolved above the freezing point, and a milky chitosan-calcium carbonate solution is obtained after centrifugal degassing. The chitosan-calcium carbonate solution was cast on a glass plate, solidified in a 25wt% K2SO4 solution at 50°C for 30 minutes to form a milky white film, and the residual chemical reagents in the film were removed with deionized water to obtain a chitosan-calcium carbonate wet film, which had a tensile strength of 0.5MPa and an elongation at break of 170%. The chitosan-calcium carbonate wet film was fixed on a plexiglass plate and dried at room temperature to obtain a white, foldable chitosan-calcium carbonate film, which had a tensile strength of 98MPa and an elongation at break of 15%.

[0057] Embodiment 11

[0058] The crab shell powder is added to a 4wt% NaOH aqueous solution and soaked at room temperature for 24h to remove protein, and then washed with deionized water. The alkali-treated crab shell powder is soaked in a 3wt% H2O2 solution, pH=9 is adjusted, and the pigment, fatty acid, etc. are removed by heating at 80°C for 40min, and then washed with deionized water and dried. A KOH aqueous solution with a mass fraction of 60wt% is prepared, and the purified chitin-calcium carbonate raw material is added to the KOH aqueous solution, and heated at 80°C for 1h to obtain a mixed solution of chitosan-calcium carbonate and alkali with a deacetylation degree of about 80%, and water and urea are added after cooling to make the KOH mass fraction in the mixed solution 16wt%, the urea mass fraction 8wt%, and the chitosan-calcium carbonate mass fraction 8wt%, and then it is frozen below the freezing point, and then thawed and dissolved above the freezing point, and a milky chitosan-calcium carbonate solution is obtained after centrifugal degassing. The chitosan-calcium carbonate solution was cast on a glass plate, solidified in a 20wt% KCl solution at 60°C for 40 minutes to form a milky white film, and the residual chemical reagents in the film were removed with deionized water to obtain a chitosan-calcium carbonate wet film, which had a tensile strength of 0.8MPa and an elongation at break of 180%. The chitosan-calcium carbonate wet film was stretched at a stretching ratio of 1 to 2.5, and then dried naturally to obtain a white, foldable chitosan-calcium carbonate film, which had a tensile strength of 108 to 256MPa and an elongation at break of 6 to 18%.

[0059] Example 12

[0060] The crab shell powder is added to a 4wt% NaOH aqueous solution and soaked at room temperature for 24h to remove protein, and then washed with deionized water. The alkali-treated crab shell powder is soaked in a 3wt% H2O2 solution, adjusted to pH=9, heated at 80°C for 40min to remove pigments, fatty acids, etc., washed with deionized water and then dried. A 60wt% KOH aqueous solution is prepared, and the purified chitin-calcium carbonate raw material is added to the KOH aqueous solution, heated at 80°C for 1h to obtain a mixed solution of chitosan-calcium carbonate and alkali with a deacetylation degree of about 80%, cooled and added with water to make the KOH mass fraction in the mixed solution 40wt%, placed at 5°C for a period of time, and then ice cubes or ice water are added to dilute the potassium hydroxide concentration to 16wt%, and the complex containing calcium carbonate and chitosan is dissolved after rapid stirring, and a chitosan-calcium carbonate complex solution is obtained after degassing, and the chitosan-calcium carbonate mass fraction is 6wt%. The chitosan-calcium carbonate solution was cast on a glass plate and solidified in a 30wt% Na2CO3 solution at 60°C for 1h to form a milky white film. The residual chemical reagents in the film were removed with deionized water to obtain a chitosan-calcium carbonate wet film, which had a tensile strength of 0.6MPa and an elongation at break of 180%. The chitosan-calcium carbonate wet film was fixed on a plexiglass plate and dried at room temperature to obtain a white, foldable chitosan-calcium carbonate film, which had a tensile strength of 102MPa and an elongation at break of 16%.

[0061] Example 13

[0062] Add crab shell powder to 4wt% NaOH aqueous solution and soak at room temperature for 24h to remove protein, wash with deionized water, soak alkali-treated crab shell powder in 3wt% H2O2 solution, adjust pH=9, heat at 40℃ for 90min to remove pigments, fatty acids, etc., wash with deionized water and dry. Prepare a 60wt% KOH aqueous solution, add the purified chitin-calcium carbonate raw material to the KOH aqueous solution, heat at 120℃ for 30min to obtain a mixed solution of chitosan-calcium carbonate and alkali with a deacetylation degree of about 90%, add water after cooling, make the KOH mass fraction in the mixed solution 60wt%, place it at 5℃ for a period of time, add ice cubes or ice water to dilute the potassium hydroxide concentration to 16wt%, quickly stir to dissolve the complex containing calcium carbonate and chitosan, degas after obtaining a chitosan-calcium carbonate complex solution, the chitosan-calcium carbonate mass fraction is 4wt%, and centrifugal degassing to obtain a milky white chitosan-calcium carbonate solution. The chitosan-calcium carbonate solution was cast on a glass plate and solidified in an ethanol solution at 5°C for 12 hours to form a milky white film. The residual chemical reagents in the film were removed with deionized water to obtain a chitosan-calcium carbonate wet film with a tensile strength of 1.2 MPa and an elongation at break of 160%. The chitosan-calcium carbonate wet film was fixed on a plexiglass plate and dried at room temperature to obtain a white, foldable chitosan-calcium carbonate film with a tensile strength of 120 MPa and an elongation at break of 14%.

[0063] Embodiment 14

[0064] Add crab shell powder to 4wt% NaOH aqueous solution and soak at room temperature for 24h to remove protein, wash with deionized water, soak alkali-treated crab shell powder in 3wt% H2O2 solution, adjust pH=9, heat at 80℃ for 40min to remove pigment, fatty acid, etc., wash with deionized water and dry. Prepare a 40wt% NaOH aqueous solution, add the purified chitosan-calcium carbonate raw material to the NaOH aqueous solution, heat at 80℃ for 40min to obtain a mixed solution of chitosan-calcium carbonate and alkali with a deacetylation degree of about 60%, add water and urea after cooling, so that the mass fraction of NaOH in the mixed solution is 12wt%, the mass fraction of urea is 6wt%, and the mass fraction of chitosan-calcium carbonate is 4wt%, stir quickly at 10℃ to dissolve, and obtain a milky chitosan-calcium carbonate solution after centrifugal degassing. The chitosan solution was poured into a perforated plate mold with a diameter of 10 mm and a height of 10 mm, and then immersed in a methanol aqueous solution with a water content of 70 wt%. After immersion for 6 hours, the chitosan gel was taken out and washed with deionized water to obtain a chitosan hydrogel with a compressive fracture stress of 3.2 MPa and a fracture strain of 68%.

[0065] Embodiment 15

[0066] The crab shell powder is added to a 4wt% NaOH aqueous solution and soaked at room temperature for 24h to remove protein, and then washed with deionized water. The alkali-treated crab shell powder is soaked in a 3wt% H2O2 solution, adjusted to pH=9, heated at 80°C for 40min to remove pigments, fatty acids, etc., washed with deionized water and then dried. A 60wt% KOH aqueous solution is prepared, and the purified chitin-calcium carbonate raw material is added to the KOH aqueous solution, heated at 80°C for 1h to obtain a mixed solution of chitosan-calcium carbonate and alkali with a deacetylation degree of about 80%, and water is added after cooling to make the KOH mass fraction in the mixed solution 35wt%, and ice cubes or ice water are added after it is placed at 5°C for a period of time to dilute the potassium hydroxide concentration to 15wt%, and the complex containing calcium carbonate and chitosan is dissolved after rapid stirring, and a chitosan-calcium carbonate complex solution is obtained after degassing, and the chitosan-calcium carbonate mass fraction is 7wt%. Add ethylene glycol diglycidyl ether in a molar ratio equivalent to 1.2 times of the chitosan monomer, stir, centrifuge and degas, then pour into a perforated plate mold with a diameter of 10 mm and a height of 10 mm. After thermal molding at 50°C, soak it in a K2CO3 aqueous solution with a salt concentration of 40wt%. After soaking for 0.5h, take out the chitosan gel and wash it with deionized water to obtain a chitosan hydrogel. The prepared chitosan hydrogel is placed in ethanol for replacement to obtain a chitosan ethanol gel, which is dried at the critical point of carbon dioxide to prepare a chitosan aerogel. The obtained chitosan aerogel is heated from room temperature to 800°C at 10°C / min, and nitrogen is used as a protective gas to obtain a nitrogen-doped porous carbon aerogel. The specific surface area of ​​the carbon aerogel obtained from the nitrogen adsorption-desorption experiment is 820m 2 / g.

[0067] The above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and changes can be made without departing from the principle of the present invention, and these improvements and changes are also regarded as the protection scope of the present invention.

Claims

1. A method for preparing a chitin / chitosan material composite with natural calcium carbonate, characterized in that: The following steps are involved: (1) Deproteinizing a raw material containing natural calcium carbonate and chitin / chitosan, and then performing an oxidative decolorization treatment with a 1-5 wt% H2O2 aqueous solution, washing, and then drying. The raw material containing natural calcium carbonate and chitin / chitosan is crab shell or shrimp shell; (2) deacetylation of the product obtained in step (1) with an alkaline aqueous solution of 20 wt% or more at 60-170° C., and obtaining a mixture of composite calcium carbonate chitin with a deacetylation degree of no more than 50% and an alkaline aqueous solution or a mixture of composite calcium carbonate chitosan with a deacetylation degree of more than 50% and an alkaline aqueous solution by controlling the deacetylation degree, and removing the alkali from the mixture and drying it to obtain composite calcium carbonate chitin or composite calcium carbonate chitosan; (3) preparing a chitin-calcium carbonate composite solution or a chitosan-calcium carbonate composite solution with an alkali concentration of 5 wt% to 30 wt%; (4) preparing a chitin material composited with natural calcium carbonate or a chitosan material composited with natural calcium carbonate, comprising any one of the following methods: A1, casting the chitin-calcium carbonate composite solution or the chitosan-calcium carbonate composite solution obtained in step (3) into a film, immersing it in a coagulant for coagulation and regeneration to obtain a chitin-calcium carbonate wet film or a chitosan-calcium carbonate wet film, washing away the chemical reagent in the wet film with water, and obtaining a chitin-calcium carbonate film or a chitosan-calcium carbonate film after stretching and drying; A2, adding the chitin-calcium carbonate composite solution or the chitosan-calcium carbonate composite solution obtained in step (3) to the chitosan-calcium carbonate composite solution; A crosslinking agent is added to the chitosan-calcium carbonate composite solution and stirred evenly, and the solution is placed in an environment close to the gelation temperature and heated to form a gel, and then immersed in a coagulant below its gelation temperature to regenerate the gel, and the chemical reagents in the gel are removed to obtain a chitin-calcium carbonate hydrogel or a chitosan-calcium carbonate hydrogel; A3, preparing a chitin-calcium carbonate hydrogel or a chitosan-calcium carbonate hydrogel, replacing the hydrogel with anhydrous ethanol or acetone for several times, and then drying with supercritical carbon dioxide to remove the liquid to obtain a chitin-calcium carbonate aerogel or a chitosan-calcium carbonate aerogel; In the step (3), the preparation of a chitosan-calcium carbonate composite solution or a chitosan-calcium carbonate composite solution with an alkali concentration of 5 wt% to 30 wt% is any one of the following methods: B1, preparing a potassium hydroxide aqueous solution with a concentration of 5 wt% to 30 wt%, adding a stabilizer, composite calcium carbonate chitosan or composite calcium carbonate chitosan, mixing evenly and freezing to below freezing point, and then thawing above freezing point to dissolve the composite calcium carbonate chitosan or composite calcium carbonate chitosan to obtain a chitosan-calcium carbonate composite solution or a chitosan-calcium carbonate composite solution; B2, preparing a potassium hydroxide aqueous solution with a concentration of 5 wt% to 30 wt%, adding a stabilizer, composite calcium carbonate chitosan or composite calcium carbonate chitosan, and continuously stirring and dissolving above freezing point and below 0°C to obtain a chitosan-calcium carbonate composite solution or a chitosan-calcium carbonate composite solution; B3, preparing a potassium hydroxide aqueous solution with a concentration of 25 wt% to 60 Composite calcium carbonate chitin or composite calcium carbonate chitosan is added to an aqueous solution of 5 wt% potassium hydroxide or sodium hydroxide, the mixed solution is placed at 0-10°C for a period of time, ice cubes or ice water are added to dilute the alkali concentration to 5 wt%-30 wt%, and the composite calcium carbonate chitin or composite calcium carbonate chitosan is dissolved after stirring to obtain a chitosan-calcium carbonate composite solution or a chitosan-calcium carbonate composite solution.

2. The method for preparing the chitin / chitosan material of composite natural calcium carbonate according to claim 1, characterized in that: In the step (1), the material-liquid ratio of the raw materials of natural calcium carbonate and chitin / chitosan to the H2O2 aqueous solution is 1:10-30, and the temperature of the oxidative decolorization treatment is 40°C to 100°C.

3. The method for preparing the chitin / chitosan material of composite natural calcium carbonate according to claim 1, characterized in that: In the step (2), the alkaline aqueous solution is a sodium hydroxide aqueous solution or a potassium hydroxide aqueous solution, and the solid-to-liquid ratio of the product to the alkaline aqueous solution is 1:10-100.

4. The method for preparing the chitin / chitosan material of composite natural calcium carbonate according to claim 1, characterized in that: The stabilizer is urea, thiourea, polyethylene glycol, and the concentration of the stabilizer in the chitin-calcium carbonate composite solution or the chitosan-calcium carbonate composite solution is 0-20 wt %.

5. The method for preparing the chitin / chitosan material of composite natural calcium carbonate according to claim 1, characterized in that: In the step (3), the concentration of the chitin-calcium carbonate composite solution or the chitosan-calcium carbonate composite solution is 1 wt% to 10 wt%.

6. The method for preparing the chitin / chitosan material of composite natural calcium carbonate according to claim 1, characterized in that: In the step (4), the coagulant is a mixed liquid of any one or more of water, saline solution, and low-viscosity organic liquid soluble in water.

7. The method for preparing the chitin / chitosan material of composite natural calcium carbonate according to claim 6, characterized in that: The salt is a salt containing monovalent cations and anions or divalent cations and anions; the water-soluble low-viscosity organic liquid is at least one of alcohols, ketones, esters, amides, and organic sulfides.

8. The method for preparing the chitin / chitosan material of composite natural calcium carbonate according to claim 1, characterized in that: In the step (4), the molar ratio of the crosslinking agent to the chitosan monomer in the composite calcium carbonate chitosan or the chitosan monomer in the composite calcium carbonate chitosan is 0-5:1, and the crosslinking agent is an epoxy compound, a glycidyl ether compound, an acrylate or an aldehyde compound.

9. The method for preparing the chitin / chitosan material of composite natural calcium carbonate according to claim 1, characterized in that: In the step (4), the drafting ratio is 1 to 2.5, and when preparing the chitosan material for composite natural calcium carbonate, the solidification regeneration temperature is (-20) to 50°C, and when preparing the chitosan material for composite natural calcium carbonate, the solidification regeneration temperature is 0-100°C.