A method for preparing a bio-based aqueous polymer binder for lithium-sulfur batteries
By grafting cysteine on chitosan, CTS-CYS bio-based aqueous polymer binder was prepared, which solved the problems of sluggish reaction kinetics and shuttle effect in lithium-sulfur batteries, improved electrochemical performance and reduced Environmental impact, achieving high efficiency performance improvement of lithium-sulfur batteries.
Patent Information
- Application Number
- CN202310365558.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-04-07
AI Technical Summary
The sluggish reaction kinetics and shuttle effect of lithium-sulfur batteries lead to a decrease in energy density, and the high toxicity and high cost of traditional organic solvent binders limit their large-scale production and performance improvement.
Chitosan (CTS) is used as the skeleton, and cysteine (CYS) is branched to its chains through room temperature amidation reaction to prepare a high-performance bio-based water-based polymer binder CTS-CYS, which has good water solubility and Mechanical properties capable of constraining polysulfides and accelerating redox reactions.
It significantly improves the reaction kinetics and rate performance of lithium-sulfur batteries, enhances electrochemical performance, improves environmental friendliness, and enables efficient binder design that does not require organic solvents.
Smart Images

Figure CN116574201B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium-sulfur battery material preparation, and relates to a method for preparing a bio-based aqueous polymer binder for lithium-sulfur batteries. Background Art
[0002] With the continuous consumption of traditional fossil energy and the intensification of global environmental pollution, the development and utilization of clean energy such as wind energy, solar energy and hydrogen energy is imperative. At the same time, countries and regions around the world have also issued a series of policy plans to promote the development and utilization of new energy. Therefore, the research and development of electrochemical energy storage devices that can efficiently store and convert various types of energy has become a feasible way to promote the development of the new energy industry. At present, lithium-ion batteries, as the most widely used energy storage device in commercialized electrochemical energy storage devices, have been maturely applied in portable devices, electric vehicles, energy storage grids and other fields. However, due to its own energy storage mechanism, the energy density of lithium-ion batteries is gradually difficult to break through the bottleneck, and its raw materials are relatively scarce and the cost is high. Therefore, it is necessary to develop a new type of secondary electrochemical energy storage device with excellent comprehensive performance, so that it can gradually replace lithium-ion batteries and lead the research and development direction of future electrochemical energy storage devices.
[0003] Compared with lithium-ion batteries, lithium-sulfur (Li-S) batteries have a capacity of up to 1675 mAh g -1 The theoretical specific capacity is over 2600Wh g -1 The theoretical energy density of lithium-sulfur batteries is 2.34 W / m, and the active material S is abundant in reserves, low in cost, and environmentally friendly. Therefore, it is expected to become a new generation of secondary electrochemical energy storage devices to replace lithium-ion batteries and has been widely studied. However, there are still many problems to be solved before lithium-sulfur batteries can be put into practical application, such as the shuttle effect of polysulfides, volume expansion of electrodes, lithium metal dendrites, slow reaction kinetics, etc. Among them, the complex multi-stage redox reaction of the active material S leads to insufficient overall battery reaction kinetics, which seriously restricts the further development of lithium-sulfur batteries and aggravates problems such as the shuttle effect. To this end, researchers have designed and prepared a variety of redox mediators and electrocatalysts, and added them as additives to the positive electrode or electrolyte of lithium-sulfur batteries to accelerate the redox kinetics of lithium-sulfur batteries. However, this additional inactive component will lead to a decrease in battery energy density, which will be more serious in large-scale energy storage devices. Therefore, improving battery reaction kinetics without affecting energy density has become a feasible direction for improving the performance of lithium-sulfur batteries.
[0004] In recent years, a series of binders designed for lithium-sulfur battery cathodes (cross-linked alginate-isosorbide, β-cyclodextrin polymer-quaternary ammonium cations, cross-linked PVP-PEI, etc.) have been shown to have good application prospects in inhibiting the shuttle effect and protecting the cathode structure. However, as a key component of the integrated lithium-sulfur battery cathode, binders still have great research potential in enhancing battery reaction kinetics. In addition, traditional binders using organic solvents will also cause difficulties in large-scale production due to their high toxicity and high cost.
[0005] Therefore, under the premise of ensuring good mechanical properties and electrode protection capabilities, how to get rid of the organic solvent system and enhance the reaction kinetics of lithium-sulfur batteries through the binder, an inherent component of the positive electrode, has become an important technical issue and feasible improvement direction in the design of new lithium-sulfur battery binders. Summary of the invention
[0006] To solve the above problems, the main purpose of the present invention is to provide a method for preparing a high-performance bio-based aqueous polymer binder for lithium-sulfur batteries, which effectively improves the redox kinetics of active substances in lithium-sulfur batteries while ensuring the excellent electrochemical performance of lithium-sulfur batteries, thereby greatly improving the reversible capacity of the positive electrode of lithium-sulfur batteries and improving its environmental friendliness. The chitosan (CTS) bio-based polymer material involved in the present invention is used as the main skeleton of the binder. From the perspective of molecular structure design, a large amount of bio-based monomer cysteine (CYS) is grafted to the CTS side chain through a convenient and low-energy room temperature amidation reaction. The obtained product binder (CTS-CYS) has good water solubility and environmental friendliness, while retaining the high viscosity and good mechanical properties of CTS, and the rich amide structure introduced can effectively constrain polysulfides, while using thiol groups to achieve the mediation acceleration of polysulfide redox reactions, and finally significantly improve the rate performance of lithium-sulfur batteries. The material prepared by the present invention can effectively accelerate the electrochemical reaction kinetics inside lithium-sulfur batteries, thereby significantly enhancing the comprehensive electrochemical performance of lithium-sulfur batteries.
[0007] The above object of the present invention is achieved through the following technical solutions:
[0008] A method for preparing a bio-based aqueous polymer binder for lithium-sulfur batteries, comprising the following steps:
[0009] (1) N-hydroxysuccinimide (NHS) and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC) are mixed in a certain mass ratio, dissolved in deionized water, and stirred continuously at room temperature to fully dissolve, thereby obtaining a mixed solution A.
[0010] (2) Add the bio-based monomer cysteine (CYS) to the mixed solution A at a certain mass ratio with NHS, continue stirring and adjust the pH value, keep stirring until the pH value is stable, then add chitosan (CTS) and stir overnight at room temperature. After the reaction is completed, a clear and transparent mixed solution B is obtained.
[0011] (3) Pour the mixed solution B into a dialysis bag that has been boiled with deionized water, seal both ends of the dialysis bag and place it in a beaker filled with deionized water to stand, replace the deionized water at regular intervals, and dialyze continuously for more than 2 days to completely remove unreacted small molecules, and then obtain a colorless and transparent product solution C.
[0012] (4) The product solution C is placed in a vacuum freeze dryer for vacuum freeze drying. After the water is completely removed, a white flocculent target product is obtained, namely, a bio-based aqueous polymer binder for lithium-sulfur batteries (CTS-CYS).
[0013] Furthermore, in step (1), the mass ratio of NHS to EDC is 1:2 to 2:1, and the total concentration of NHS and EDC in the mixed solution A is 10 to 30 g / L.
[0014] Furthermore, in step (2), the mass ratio of CYS to NHS is 1:2 to 2:1.
[0015] Furthermore, in step (2), the molecular weight of the CTS is 100,000 to 600,000.
[0016] Furthermore, in step (2), the mass ratio of CTS to CYS is 2:1 to 1:2.
[0017] Furthermore, in step (2), the pH value is 3-5.
[0018] Furthermore, in step (3), the time interval between the regular time intervals is 3 to 6 hours.
[0019] Beneficial effects of the present invention:
[0020] The preparation method of the high-performance bio-based water-based polymer binder of the present invention adopts the natural polymer CTS with good mechanical properties as the polymer skeleton structure, and from the perspective of molecular structure design, a large amount of cysteine (CYS) is grafted to the CTS side chain through a convenient and low-energy room temperature amidation reaction, thereby creating a new type of high-performance bio-based water-based polymer binder CTS-CYS. It has good water solubility and environmental friendliness, while retaining the high viscosity and good mechanical properties of CTS, and the rich amide structure introduced can effectively constrain polysulfides to avoid the shuttle effect, and its rich thiol groups can mediate and accelerate the redox reaction of polysulfides, thereby solving the problems of the environmental pollution of traditional binders and the slow reaction kinetics of lithium-sulfur batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the scanning electron microscope image of the positive electrode prepared with CTS-CYS binder.
[0022] Figure 2 The figure is a bar graph comparing the discharge specific capacities at different current densities after assembling batteries with electrodes prepared from 5 embodiments (CTS-CYS binder), comparative example 1 (physically mixed CTS+CYS binder) and comparative example 2 (PVDF commercial binder). DETAILED DESCRIPTION
[0023] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and technical solutions.
[0024] In the embodiment of the present invention, the prepared bio-based aqueous polymer binder is used as the positive electrode material of the lithium-sulfur battery, and the lithium-sulfur battery is assembled. The lithium-sulfur battery positive electrode sheet involved is composed of an active material (carbon-sulfur composite material), a conductive agent (Super P) and a binder, and the ratio of the three is 7:2:1.
[0025] Example 1
[0026] (1) NHS and EDC in a mass ratio of 1:1 were added to a glass beaker and dissolved in deionized water to prepare a solution with a total concentration of 20 g / L. After sufficient dissolution, CYS was added to the solution at a mass ratio of CYS:NHS=1:1, and the pH value of the mixed solution was adjusted to 3 under the detection of a pH meter. After the pH value was stabilized, CTS with a molecular weight of about 100,000 was added to the mixed solution at a mass ratio of CTS:CYS=1:1, and then stirred overnight at room temperature to obtain a clear and transparent colorless solution;
[0027] (2) The obtained solution was added to a dialysis bag that had been boiled with deionized water, and the two ends of the dialysis bag were sealed and placed in a 1L beaker filled with deionized water. The deionized water was replaced every 6 hours, and the dialysis was continued for 3 days to completely remove the unreacted small molecules, and then a colorless and transparent product solution was obtained. The product solution was placed in a vacuum freeze dryer for treatment, and after the water was completely removed, a white flocculent target product was obtained, which was a high-performance water-based polymer binder (CTS-CYS) prepared from all bio-based materials;
[0028] (3) 0.75 g of elemental sulfur was dissolved in 10 ml of CS2, and then 0.25 g of rGO was added and ultrasonicated for 3 hours to make it uniformly dispersed. The mixture was heated and stirred at 60 °C for 1 hour to ensure complete removal of CS2, and then the solid was heated at 155 °C for 10 hours and then at 200 °C for 2 hours to obtain rGO@S;
[0029] (4) RGO@S, Super P, and CTS-CYS were uniformly ground in a small amount of deionized water according to a mass ratio of 7:2:1, and the obtained black slurry was evenly coated on a carbon-coated aluminum foil, dried in a vacuum oven at 60°C for 24 hours, and cut into pieces after the electrode piece was completely cooled and dried to obtain a circular lithium-sulfur battery positive electrode sheet with a diameter of 14 mm;
[0030] (5) The assembly type of lithium-sulfur batteries is uniformly CR2032 button cells, and the entire assembly process is carried out in a glove box filled with argon. The assembly order is positive electrode shell, positive electrode prepared by CTS-CYS, ether-based electrolyte (1.0M LiTFSI in DOL:DME=1:1Vol%with 2.0%LiNO3), single-layer polypropylene separator (PP, Celgard 2500), lithium metal negative electrode, stainless steel gasket, stainless steel spring and negative electrode shell.
[0031] In step (5), the lithium metal negative electrode used in the battery has a diameter of 15.5 mm, the single-layer polypropylene separator has a diameter of 19 mm, and the sulfur surface loading in each circular positive electrode sheet with a diameter of 14 mm is maintained at 1.0-1.5 mg / cm 2 The ratio of electrolyte addition to active material was controlled at 15 μL / mg.
[0032] Example 2
[0033] (1) NHS and EDC in a mass ratio of 1:1 were added to a glass beaker and dissolved in deionized water to prepare a solution with a total concentration of 20 g / L. After sufficient dissolution, CYS was added to the solution at a mass ratio of CYS:NHS=1:1, and the pH value of the mixed solution was adjusted to 4 under the detection of a pH meter. After the pH value was stabilized, CTS with a molecular weight of about 600,000 was added to the mixed solution at a mass ratio of CTS:CYS=1:2, and then stirred overnight at room temperature to obtain a clear and transparent colorless solution;
[0034] (2) The obtained solution was added to a dialysis bag that had been boiled with deionized water, and the two ends of the dialysis bag were sealed and placed in a 1L beaker filled with deionized water. The deionized water was replaced every 3 hours, and the dialysis was continued for 3 days to completely remove the unreacted small molecules, and then a colorless and transparent product solution was obtained. The product solution was placed in a vacuum freeze dryer for treatment, and after the water was completely removed, a white flocculent target product was obtained, which was a high-performance water-based polymer binder (CTS-CYS) prepared from all bio-based materials;
[0035] (3) 0.75 g of elemental sulfur was dissolved in 10 ml of CS2, and then 0.25 g of rGO was added and ultrasonicated for 3 hours to make it uniformly dispersed. The mixture was heated and stirred at 60 °C for 1 hour to ensure complete removal of CS2, and then the solid was heated at 155 °C for 10 hours and then at 200 °C for 2 hours to obtain rGO@S;
[0036] (4) RGO@S, Super P, and CTS-CYS were uniformly ground in a small amount of deionized water according to a mass ratio of 7:2:1, and the obtained black slurry was evenly coated on a carbon-coated aluminum foil, dried in a vacuum oven at 60°C for 24 hours, and cut into pieces after the electrode piece was completely cooled and dried to obtain a circular lithium-sulfur battery positive electrode sheet with a diameter of 14 mm;
[0037] (5) The assembly type of lithium-sulfur batteries is uniformly CR2032 button cells, and the entire assembly process is carried out in a glove box filled with argon. The assembly order is positive electrode shell, positive electrode prepared by CTS-CYS, ether-based electrolyte (1.0M LiTFSI in DOL:DME=1:1Vol%with 2.0%LiNO3), single-layer polypropylene separator (PP, Celgard 2500), lithium metal negative electrode, stainless steel gasket, stainless steel spring and negative electrode shell.
[0038] Example 3
[0039] (1) NHS and EDC in a mass ratio of 1:1 were added to a glass beaker and dissolved in deionized water to prepare a solution with a total concentration of 20 g / L. After sufficient dissolution, CYS was added to the solution in a mass ratio of CYS:NHS=1:1, and the pH value of the mixed solution was adjusted to 5 under the detection of a pH meter. After the pH value was stabilized, CTS with a molecular weight of about 300,000 was added to the mixed solution in a mass ratio of CTS:CYS=2:1, and then stirred overnight at room temperature to obtain a clear and transparent colorless solution;
[0040] (2) Add the obtained solution to a dialysis bag that has been boiled with deionized water, seal both ends of the dialysis bag and place it in a 1L beaker filled with deionized water. Replace the deionized water every 5 hours, and dialyze for 3 consecutive days to completely remove unreacted small molecules, and then obtain a colorless and transparent product solution. Place the product solution in a vacuum freeze dryer for treatment. After the water is completely removed, a white flocculent target product is obtained, which is a high-performance water-based polymer binder (CTS-CYS) prepared from all bio-based materials;
[0041] (3) 0.75 g of elemental sulfur was dissolved in 10 ml of CS2, and then 0.25 g of rGO was added and ultrasonicated for 3 hours to make it uniformly dispersed. The mixture was heated and stirred at 60 °C for 1 hour to ensure complete removal of CS2, and then the solid was heated at 155 °C for 10 hours and then at 200 °C for 2 hours to obtain rGO@S;
[0042] (4) RGO@S, Super P, and CTS-CYS were uniformly ground in a small amount of deionized water according to a mass ratio of 7:2:1, and the obtained black slurry was evenly coated on a carbon-coated aluminum foil, dried in a vacuum oven at 60°C for 24 hours, and cut into pieces after the electrode piece was completely cooled and dried to obtain a circular lithium-sulfur battery positive electrode sheet with a diameter of 14 mm;
[0043] (5) The assembly type of lithium-sulfur batteries is uniformly CR2032 button cells, and the entire assembly process is carried out in a glove box filled with argon. The assembly order is positive electrode shell, positive electrode prepared by CTS-CYS, ether-based electrolyte (1.0M LiTFSI in DOL:DME=1:1Vol%with 2.0%LiNO3), single-layer polypropylene separator (PP, Celgard 2500), lithium metal negative electrode, stainless steel gasket, stainless steel spring and negative electrode shell.
[0044] Example 4
[0045] (1) NHS and EDC in a mass ratio of 1:2 were added to a glass beaker and dissolved in deionized water to prepare a solution with a total concentration of 10 g / L. After sufficient dissolution, CYS was added to the solution in a mass ratio of CYS:NHS=2:1. CYS was added to the solution, and the pH value of the mixed solution was adjusted to 4 under the detection of a pH meter. After the pH value was stable, CTS with a molecular weight of about 600,000 was added to the mixed solution in a mass ratio of CTS:CYS=1:2, and then stirred overnight at room temperature to obtain a clear and transparent colorless solution;
[0046] (2) The obtained solution was added to a dialysis bag that had been boiled with deionized water, and the two ends of the dialysis bag were sealed and placed in a 1L beaker filled with deionized water. The deionized water was replaced every 3 hours, and the dialysis was continued for 3 days to completely remove the unreacted small molecules, and then a colorless and transparent product solution was obtained. The product solution was placed in a vacuum freeze dryer for treatment, and after the water was completely removed, a white flocculent target product was obtained, which was a high-performance water-based polymer binder (CTS-CYS) prepared from all bio-based materials;
[0047] (3) 0.75 g of elemental sulfur was dissolved in 10 ml of CS2, and then 0.25 g of rGO was added and ultrasonicated for 3 hours to make it uniformly dispersed. The mixture was heated and stirred at 60 °C for 1 hour to ensure complete removal of CS2, and then the solid was heated at 155 °C for 10 hours and then at 200 °C for 2 hours to obtain rGO@S;
[0048] (4) RGO@S, Super P, and CTS-CYS were uniformly ground in a small amount of deionized water according to a mass ratio of 7:2:1, and the obtained black slurry was evenly coated on a carbon-coated aluminum foil, dried in a vacuum oven at 60°C for 24 hours, and cut into pieces after the electrode piece was completely cooled and dried to obtain a circular lithium-sulfur battery positive electrode sheet with a diameter of 14 mm;
[0049] (5) The assembly type of lithium-sulfur batteries is uniformly CR2032 button cells, and the entire assembly process is carried out in a glove box filled with argon. The assembly order is positive electrode shell, positive electrode prepared by CTS-CYS, ether-based electrolyte (1.0M LiTFSI in DOL:DME=1:1Vol%with 2.0%LiNO3), single-layer polypropylene separator (PP, Celgard 2500), lithium metal negative electrode, stainless steel gasket, stainless steel spring and negative electrode shell.
[0050] Example 5
[0051] (1) NHS and EDC in a mass ratio of 2:1 were added to a glass beaker and dissolved in deionized water to prepare a solution with a total concentration of 30 g / L. After sufficient dissolution, CYS was added to the solution in a mass ratio of CYS:NHS=1:2, and the pH value of the mixed solution was adjusted to 4 under the detection of a pH meter. After the pH value was stabilized, CTS with a molecular weight of about 600,000 was added to the mixed solution in a mass ratio of CTS:CYS=1:2, and then stirred overnight at room temperature to obtain a clear and transparent colorless solution;
[0052] (2) The obtained solution was added to a dialysis bag that had been boiled with deionized water, and the two ends of the dialysis bag were sealed and placed in a 1L beaker filled with deionized water. The deionized water was replaced every 3 hours, and the dialysis was continued for 3 days to completely remove the unreacted small molecules, and then a colorless and transparent product solution was obtained. The product solution was placed in a vacuum freeze dryer for treatment, and after the water was completely removed, a white flocculent target product was obtained, which was a high-performance water-based polymer binder (CTS-CYS) prepared from all bio-based materials;
[0053] (3) 0.75 g of elemental sulfur was dissolved in 10 ml of CS2, and then 0.25 g of rGO was added and ultrasonicated for 3 hours to make it uniformly dispersed. The mixture was heated and stirred at 60 °C for 1 hour to ensure complete removal of CS2, and then the solid was heated at 155 °C for 10 hours and then at 200 °C for 2 hours to obtain rGO@S;
[0054] (4) RGO@S, Super P, and CTS-CYS were uniformly ground in a small amount of deionized water according to a mass ratio of 7:2:1, and the obtained black slurry was evenly coated on a carbon-coated aluminum foil, dried in a vacuum oven at 60°C for 24 hours, and cut into pieces after the electrode piece was completely cooled and dried to obtain a circular lithium-sulfur battery positive electrode sheet with a diameter of 14 mm;
[0055] (5) The assembly type of lithium-sulfur batteries is uniformly CR2032 button cells, and the entire assembly process is carried out in a glove box filled with argon. The assembly order is positive electrode shell, positive electrode prepared by CTS-CYS, ether-based electrolyte (1.0M LiTFSI in DOL:DME=1:1Vol%with 2.0%LiNO3), single-layer polypropylene separator (PP, Celgard 2500), lithium metal negative electrode, stainless steel gasket, stainless steel spring and negative electrode shell.
[0056] Comparative Example 1
[0057] A CTS+CYS binder for lithium-sulfur batteries is manufactured by the following specific process:
[0058] (1) Dissolve 2 g CYS and 1 g CTS in 200 ml deionized water and stir overnight at room temperature to obtain a clear, colorless solution.
[0059] (2) The product solution is placed in a vacuum freeze dryer for treatment. After the water is completely removed, a light yellow powdery target product is obtained, which is a CTS and CYS mixture binder (CTS+CYS) that is uniformly mixed by physical means without chemical reaction.
[0060] (3) 0.75 g of elemental sulfur was dissolved in 10 ml of CS2, and then 0.25 g of rGO was added and ultrasonicated for 3 hours to make it uniformly dispersed. The mixture was heated and stirred at 60 °C for 1 hour to ensure complete removal of CS2, and then the solid was heated at 155 °C for 10 hours and then at 200 °C for 2 hours to obtain rGO@S;
[0061] (4) RGO@S, Super P, and CTS+CYS were uniformly ground in a small amount of deionized water according to a mass ratio of 7:2:1, and the obtained black slurry was evenly coated on a carbon-coated aluminum foil, dried in a vacuum oven at 60°C for 24 hours, and cut into pieces after the electrode piece was completely cooled and dried to obtain a circular lithium-sulfur battery positive electrode sheet with a diameter of 14 mm;
[0062] (5) The assembly type of lithium-sulfur batteries is uniformly CR2032 button cells, and the entire assembly process is carried out in a glove box filled with argon. The assembly order is positive electrode shell, positive electrode prepared by CTS+CYS, ether-based electrolyte (1.0M LiTFSI in DOL:DME=1:1Vol%with 2.0%LiNO3), single-layer polypropylene separator (PP, Celgard 2500), lithium metal negative electrode, stainless steel gasket, stainless steel spring and negative electrode shell.
[0063] Comparative Example 2
[0064] The other parts are the same as those of Comparative Example 1, except that: the steps of preparing the CTS+CYS mixed binder in steps (1) and (2) are no longer performed. In the process of preparing the electrode slurry in step (4), the binder is no longer the CTS+CYS mixed binder, but the commercial binder PVDF is selected for the subsequent preparation of the positive electrode and assembly of the battery.
[0065] Performance test and result comparison:
[0066] Comparison of the discharge specific capacity at different current densities after assembling batteries with electrodes prepared in the five examples (CTS-CYS binder), comparative example 1 (physically mixed CTS+CYS binder) and comparative example 2 (PVDF commercial binder) Figure 2 shown.
[0067] The electrochemical test results are shown in Table 1, which are the discharge specific capacities at 0.1C and 2C after assembling batteries with electrodes prepared in the five embodiments (CTS-CYS binder), Comparative Example 1 (physically mixed CTS+CYS binder) and Comparative Example 2 (PVDF commercial binder), and the reversible specific capacities after 200 cycles at 0.5C.
[0068] Table 1 Test results
[0069]
[0070] The test results show that the cycle stability and mass specific capacity of lithium-sulfur batteries assembled with CTS-CYS binder prepared by grafting and CTS+CYS binder obtained by physical mixing are better than those of commercial binder PVDF. Figure 1 The scanning electron micrograph of the electrode prepared by the CTS-CYS binder after cycling shows that the CTS-CYS binder has good structural protection for the positive electrode. The results show that the initial specific capacity of the lithium-sulfur battery assembled by the CTS-CYS binder obtained by grafting CYS on CTS can reach 1202 mAh g -1 , achieving the goal of improving the reaction kinetics of lithium-sulfur batteries through binders, thereby improving the comprehensive electrochemical performance of lithium-sulfur batteries.
Claims
1. A lithium-sulfur battery, characterized in that: The preparation method thereof comprises the following steps: (1) NHS and EDC in a mass ratio of 1:1 were added into a glass beaker and dissolved in deionized water to prepare a solution with a total concentration of 20 g / L. After sufficient dissolution, CYS was added into the solution in a mass ratio of CYS:NHS=1:1, and the pH value of the mixed solution was adjusted to 4 under the detection of a pH meter. After the pH value was stabilized, CTS with a molecular weight of 600000 was added into the mixed solution in a mass ratio of CTS:CYS=1:2, and then stirred overnight at room temperature to obtain a clear and transparent colorless solution; wherein NHS is N-hydroxysuccinimide, EDC is 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, CYS is cysteine, and CTS is chitosan; (2) The obtained solution was added to a dialysis bag that had been boiled with deionized water. The two ends of the dialysis bag were sealed and placed in a 1L beaker filled with deionized water. The deionized water was replaced every 3 hours. The dialysis was continued for 3 days to completely remove the unreacted small molecules, and then a colorless and transparent product solution was obtained. The product solution was placed in a vacuum freeze dryer for treatment. After the water was completely removed, a white flocculent target product was obtained, which was a high-performance water-based polymer binder CTS-CYS prepared from all-biobased materials. (3) 0.75 g of elemental sulfur was dissolved in 10 ml of CS2, and then 0.25 g of rGO was added and ultrasonicated for 3 h to make it uniformly dispersed; the mixture was heated and stirred at 60 °C for 1 h to ensure complete removal of CS2, and then the solid was heated at 155 °C for 10 h and then at 200 °C for 2 h to obtain rGO@S; (4) RGO@S, Super P, and CTS-CYS were uniformly ground in a small amount of deionized water according to a mass ratio of 7:2:1, and the obtained black slurry was evenly coated on a carbon-coated aluminum foil, dried in a vacuum oven at 60°C for 24 hours, and cut into pieces after the electrode piece was completely cooled and dried to obtain a circular lithium-sulfur battery positive electrode sheet with a diameter of 14 mm; (5) The assembly type of lithium-sulfur batteries is uniformly CR2032 button cells, and the entire assembly process is carried out in a glove box filled with argon; the assembly order is positive electrode shell, positive electrode prepared by CTS-CYS, ether-based electrolyte, single-layer polypropylene diaphragm, lithium metal negative electrode, stainless steel gasket, stainless steel spring and negative electrode shell. The ether-based electrolyte is 1.0M LiTFSI in a volume ratio of DOL:DMF=1:1, and contains 2.0% LiNO3.
Citation Information
Patent Citations
Binder for positive electrode of lithium-sulfur battery and preparation method of binder
CN106505204A
Lithium-sulfur battery binder and preparation method thereof, and use method thereof, and lithium-sulfur battery
CN110518244A
Preparation method of crosslinking-type aqueous binder for lithium-ion batteries incorporating slurry coating and drying process
US20200014029A1
Rechargeable copper and sulfur based electrodes for electrochemical applications
WO2019028363A1
Cited By
Binder for sulfur-based cathodes and use thereof
CN122832639A