A solvent-processed plant fiber household paper and preparation method thereof
The slurry prepared through the solvent method and the high-concentration refining process combined with needle and broad-leaf chemical pulp solves the problems of heavy metal ions and limited raw materials in traditional domestic papers, and realizes high-quality domestic paper production and improves the The thickness and feel of the paper.
Patent Information
- Application Number
- CN202310702121.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-06-14
AI Technical Summary
The slurry caused by the traditional alkali and acid pulping process used in the production of existing domestic paper contains heavy metal ions, which is relatively safe, and has limited source of raw materials, high papermaking costs, and the paper-forming thickness and feel are average.
The preparation method of plant fiber daily paper by solvent method is used. The slurry prepared by high-concentration refining process does not contain heavy metal ions and has low content of other metal ions. It combines needles and broad-leaf chemical slurry, and uses alcohols, organic acids or esters. Solvent-like pretreatment, combined with wet strength agent and softener, is fabricated and dried to form high-quality domestic paper.
The preparation of slurry without heavy metal ions is realized, the looseness and feel of the paper is improved, the cost of raw materials is reduced, and the safety and quality of the product is improved.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to a solvent-processed plant fiber household paper and a preparation method thereof, belonging to the technical field of papermaking. Background Art
[0002] As a necessary consumer product, the raw materials and varieties of household paper are gradually expanding. From the initial toilet paper to the current high-end series of baby paper, cream paper, etc., the requirements for performance and quality of household paper are increasing day by day.
[0003] Chinese Patent 201310498141.6 proposed a process for producing household paper using hardwood chemical pulp, softwood chemical pulp and high-yield pulp in a multi-layer composite manner, expanding the field of raw materials for household paper. Chinese Patent 201680056975.3 proposed using hardwood and softwood kraft pulp, and adding fatty acid ester compounds and fatty acid amide compounds to obtain soft-touch household paper. Chinese Patent 202210091099.5 uses natural chemical wood pulp, natural reed pulp and PET fiber, combined with various papermaking chemicals to produce environmentally friendly sanitary toilet paper, and its strength is effectively improved.
[0004] At present, the mainstream technology in the field of household paper is to use bleached, natural chemical wood pulp or chemical straw pulp, and occasionally add viscose fiber and other composite fibers. The source of raw materials is limited, and the price has remained high in recent years, resulting in high papermaking costs. The pulp obtained by traditional alkaline and acid pulping processes contains some heavy metal ions and is less safe. In addition, the bulk and feel of traditional papermaking are average. Summary of the invention
[0005] In order to solve the above problems, a solvent-based plant fiber household paper and a preparation method thereof are provided. Compared with the pulp obtained by the traditional alkaline and acid pulping processes, the pulp prepared in the present application does not contain any heavy metal ions and has a lower content of other metal ions, is safer, and is more suitable for the production of household paper. At the same time, its hemicellulose and lignin contents are lower than those of traditional chemical pulp. When used in conjunction with a high-concentration pulping process, the finished paper has a higher bulk thickness and a better feel, thereby greatly improving the product quality.
[0006] According to one aspect of the present application, a method for preparing solvent-processed plant fiber household paper is provided, comprising the following steps:
[0007] (1) Solvent-based cellulose pretreatment: Refining is performed using a high-consistency refiner. Solvent-based cellulose is prepared using any solvent including organic acids, alcohols or esters;
[0008] (2) Pretreatment of coniferous and broadleaf chemical pulp: coniferous chemical pulp is refined by two-stage combined pulping, and broadleaf chemical pulp is refined by a high-consistency refiner;
[0009] (3) pulping: according to weight percentage, the coniferous chemical pulp is 10-20%, the broadleaf chemical pulp is 0-20%, and the solvent-based cellulose is 70-90%. After the pulping is completed, a wet strength agent or a combination of a wet strength agent and a softener is added, and the mixture is evenly mixed before papermaking;
[0010] (4) Dehydration and drying: The wet paper sheets made by the papermaking machine are dehydrated and then dried;
[0011] (5) Creping and rolling: The dried paper sheet is creped at a creping scraper, and the creped paper sheet is rolled up to obtain the solvent-processed plant fiber household paper.
[0012] Specifically, the preparation method of solvent-based cellulose includes the following steps: mixing wood chips, bamboo chips and straw, and then boiling them at 50-200°C for 30-120 minutes using an alcohol (including but not limited to methanol, ethanol, butanediol, propylene glycol), or an organic acid (including but not limited to formic acid, acetic acid), or an ester (including but not limited to ethyl acetate) aqueous solution, and then washing the pulp and performing single-stage or multi-stage combined bleaching using a bleaching agent (including but not limited to hydrogen peroxide, ozone, chlorine dioxide) to obtain the cellulose.
[0013] Specifically, the preparation method of alcohol solvent cellulose includes the following steps: mixing wood chips, bamboo chips and straw, adding water and 80% mass concentration of 1,4-butanediol aqueous solution, cooking at 80-150°C for 20-70 minutes, filtering and bleaching the solid part with hydrogen peroxide to obtain cellulose.
[0014] Specifically, the preparation method of organic acid solvent cellulose includes the following steps: mixing wood chips, bamboo chips and straw, adding water and a formic acid aqueous solution with a mass concentration of 50-90%, cooking at 60-120°C for 20-70 minutes, filtering and bleaching the solid part with hydrogen peroxide to obtain the cellulose.
[0015] Optionally, in step (1), the pulping concentration is 15-25%, and the pulp beating degree is controlled to be 35-45°SR.
[0016] Optionally, in step (2), the pulping concentration of coniferous chemical pulp is 3-4%, and the pulping beating degree is controlled at 25-35°SR; the pulping concentration of broadleaf chemical pulp is 15-25%, and the pulping beating degree is controlled at 20-30°SR.
[0017] Optionally, in step (3), the amount of wet strength agent added is 1-10% of the absolute dry mass of the total slurry, the amount of softener added is 0-1.5% of the absolute dry mass of the total slurry, and the basis weight of the paper sheet is 10-20 g / m 2 .
[0018] Optionally, the wet strength agent is any one of polyamide epichlorohydrin, urea-formaldehyde resin, dialdehyde starch, and glyoxal polyamide resin.
[0019] Optionally, the softener is any one of quaternary ammonium salt type, silicone type, water-based polyurethane, and polyethylene type.
[0020] Optionally, in step (4), the wet paper sheets are dehydrated in turn by a vacuum suction box and a vacuum roller, and then dried by a drying cylinder, and the dryness of the paper sheets is controlled to be 88%-95% when leaving the drying cylinder.
[0021] Preferably, the drying temperature is 110-160°C.
[0022] Optionally, in step (5), the wrinkling rate is controlled at 20-30%.
[0023] According to another aspect of the present application, a solvent-processed plant fiber household paper is also provided, which is prepared by any of the above methods.
[0024] The beneficial effects of this application include but are not limited to:
[0025] 1. According to the solvent-based plant fiber daily paper preparation method of the present application, the pulp prepared in the present application does not contain any heavy metal ions and has a lower content of other metal ions than the pulp obtained by the traditional alkaline and acid pulping processes, is safer, and is more suitable for the production of daily paper. At the same time, its hemicellulose and lignin content are lower than those of traditional chemical pulp. In combination with the use of a high-concentration pulping process, the finished paper has a higher bulkiness and a better feel, greatly improving the product quality.
[0026] 2. According to the solvent-based plant fiber household paper preparation method of the present application, the cellulose pulp obtained by the solvent method has a low content of hemicellulose and lignin in the pulp, and is combined with high-concentration pulping to enable the fibers to be better fibrillated and avoid large-scale cutting. While obtaining high strength and thickness, it can also increase the bulk and improve the feel of use.
[0027] 3. According to the method for preparing solvent-based plant fiber household paper of the present application, by subjecting broadleaf chemical pulp to high-concentration pulping, the fibers are rubbed against each other to form fibers, which is beneficial to improving wet strength and bulk.
[0028] 4. According to the solvent-based plant fiber household paper preparation method of the present application, the present application utilizes a variety of raw materials such as wood, straw, wheat straw, reed, bamboo, corn straw, etc. to obtain raw materials for pulping and papermaking through solvent pulping. The raw materials are widely available, solving the problems of raw material shortage and high prices.
[0029] 5. According to the method for preparing solvent-based plant fiber household paper of the present application, by limiting the ratio of solvent-based cellulose pulp, coniferous chemical pulp and broadleaf chemical pulp, the paper sheet can obtain better bulk and hand feel experience on the basis of sufficient strength. Coniferous pulp is the skeleton and support of the paper sheet, which can provide a strength basis, but its bulk is low and its hardness is high. Adding a large amount of it will cause the uniformity of the paper sheet to decrease, and the paper will become hard, affecting the user experience; broadleaf pulp provides uniform short fibers, improves the uniformity of the paper, and takes into account strength and softness to a certain extent; solvent-based cellulose mainly provides bulk and softness. The combination of the three achieves a balance between strength and softness, strengthens the bonding between the pulp fibers, and is beneficial to improving the performance of the paper.
[0030] 6. According to the solvent-based plant fiber household paper preparation method of the present application, by limiting the amount of wet strength agent added, on the one hand, it is beneficial to ensure the wet strength of the paper sheet and avoid it being easily broken by water. On the other hand, it mainly ensures that during the papermaking process, the wet strength agent is prevented from causing excessive flocculation of the pulp and affecting the uniformity of the paper sheet; by limiting the softener, the softener is effective and avoids damage to the strength of the paper, which can bring a more comfortable hand feel. Excessive dosage will cause low paper sheet strength. DETAILED DESCRIPTION
[0031] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0032] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar or equivalent to the described content can be applied to the method of the present invention. The preferred implementation methods and materials described in this patent are for demonstration purposes only.
[0033] The embodiment uses reed solvent pulp as an example to illustrate the production and preparation process, and uses different ratios and amounts of chemical addition to obtain finished paper, and compares its performance with the mainstream chemical straw pulp household paper sold in the market.
[0034] Example 1: Tissue Paper 1#
[0035] The preparation method comprises the following steps:
[0036] (1) using a high-consistency refiner for refining, the solvent-based cellulose is reed pulp prepared with an organic acid solvent, the refining concentration is 20%, and the beating degree is 43°SR;
[0037] (2) The coniferous chemical pulp adopts two-stage combined refining, the bleached coniferous chemical pulp refining concentration is 3.62%, and the beating degree is 29°SR;
[0038] (3) Pulping: 85% solvent-processed reed pulp, 15% bleached coniferous chemical pulp, paper weight 16.8g / m 2 The wet strength agent is polyamide epichlorohydrin, the addition amount is 2% of the total slurry absolute dry mass, no softener is added, and papermaking is carried out after mixing evenly;
[0039] (4) Dehydration and drying: The wet paper sheets are dehydrated in a vacuum suction box and vacuum rollers, and then dried by a drying cylinder. The dryness of the paper sheets is controlled at 94% when they leave the drying cylinder.
[0040] (5) Crinkling and rolling: The dried paper sheet is wrinkled at a wrinkling scraper with a wrinkling rate of 25%. The wrinkled paper sheet is rolled up to obtain the solvent-processed plant fiber household paper No. 1.
[0041] Example 2: Tissue Paper 2#
[0042] The preparation method comprises the following steps:
[0043] (1) using a high-consistency refiner for refining, the solvent-based cellulose is a reed pulp prepared from an organic alcohol solvent, the refining concentration is 18%, and the beating degree is 40°SR;
[0044] (2) The coniferous chemical pulp adopts two-stage combined refining, the bleached coniferous chemical pulp refining concentration is 3.53%, and the beating degree is 27°SR;
[0045] (3) Pulping: 80% solvent-processed reed pulp, 20% bleached coniferous chemical pulp, paper weight 15.8g / m 2 , urea-formaldehyde resin is used as wet strength agent, and the addition amount is 1% of the absolute dry weight of the total slurry. No softener is added, and papermaking is carried out after mixing evenly;
[0046] (4) Dehydration and drying: The wet paper sheets are dehydrated in a vacuum suction box and vacuum rollers, and then dried by a drying cylinder. The dryness of the paper sheets is controlled at 93% when they leave the drying cylinder.
[0047] (5) Crinkling and rolling: The dried paper sheet is wrinkled at a wrinkling scraper with a wrinkling rate of 25%. The wrinkled paper sheet is rolled up to obtain the solvent-processed plant fiber household paper No. 2.
[0048] Example 3: Tissue Paper 3#
[0049] The preparation method comprises the following steps:
[0050] (1) using a high-consistency refiner for pulping, the solvent-based cellulose is a reed pulp prepared with an organic acid solvent, the pulping concentration is 22%, and the beating degree is 45°SR;
[0051] (2) The coniferous chemical pulp adopts two-stage combined refining, the bleached coniferous chemical pulp refining concentration is 3.31%, and the beating degree is 28°SR;
[0052] (3) Pulping: 90% solvent-processed reed pulp, 10% bleached coniferous chemical pulp, paper weight 16.2g / m 2 The wet strength agent uses glyoxal polyamide resin, the addition amount is 1.5% of the total slurry absolute dry mass, the softener is quaternary ammonium salt type, the addition amount is 0.5% of the total slurry absolute dry mass, and the papermaking is carried out after mixing evenly;
[0053] (4) Dehydration and drying: The wet paper sheets are dehydrated in turn by vacuum suction boxes and vacuum rollers, and then dried by drying cylinders. The dryness of the paper sheets is controlled at 95% when they leave the drying cylinders.
[0054] (5) Crinkling and rolling: The dried paper sheet is wrinkled at a wrinkling scraper with a wrinkling rate of 23%. The wrinkled paper sheet is rolled up to obtain the solvent-processed plant fiber household paper No. 3.
[0055] Example 4: Tissue Paper 4#
[0056] The preparation method comprises the following steps:
[0057] (1) using a high-consistency refiner for pulping, the solvent-based cellulose is a reed pulp prepared from an organic alcohol solvent, the pulping concentration is 20%, and the beating degree is 44°SR;
[0058] (2) The coniferous chemical pulp is refined by a two-stage combined refiner, and the broadleaf chemical pulp is refined by a high-consistency refiner. The bleached coniferous chemical pulp is refined at a concentration of 3.41% and a beating degree of 28°SR, and the bleached broadleaf pulp is refined at a concentration of 20% and a beating degree of 23°SR;
[0059] (3) Pulping: Pulping ratio: 70% solvent-processed reed pulp, 10% bleached coniferous chemical pulp, 20% bleached broadleaf chemical pulp, paper weight 15.7g / m 2 The wet strength agent is polyamide epichlorohydrin type, the addition amount is 2% of the total slurry absolute dry mass, the softener is quaternary ammonium salt type, the addition amount is 0.5% of the total slurry absolute dry mass, and the papermaking is carried out after mixing evenly;
[0060] (4) Dehydration and drying: The wet paper sheets are dehydrated in a vacuum suction box and vacuum rollers, and then dried by a drying cylinder. The dryness of the paper sheets is controlled at 94% when they leave the drying cylinder.
[0061] (5) Crinkling and rolling: The dried paper sheet is wrinkled at a wrinkling scraper with a wrinkling rate of 23%. The wrinkled paper sheet is rolled up to obtain the solvent-processed plant fiber household paper No. 4.
[0062] Comparative Example 1 Comparison of tissue paper 1#
[0063] The preparation method comprises the following steps:
[0064] (1) using double disc mill at low concentration, solvent cellulose is reed pulp prepared by organic alcohol solvent, the pulping concentration is 3.5%, and the beating degree is 42°SR;
[0065] (2) The coniferous chemical pulp adopts two-stage combined refining, the bleached coniferous chemical pulp refining concentration is 3.59%, and the beating degree is 27°SR;
[0066] (3) Pulping: Pulping ratio: 90% solvent-processed reed pulp, 10% bleached coniferous chemical pulp, paper weight 15.9g / m 2 The wet strength agent is polyamide epichlorohydrin type, the addition amount is 1.5% of the total slurry absolute dry mass, the softener is quaternary ammonium salt type, the addition amount is 0.5% of the total slurry absolute dry mass, and the papermaking is carried out after mixing evenly;
[0067] (4) Dehydration and drying: The wet paper sheets are dehydrated in turn by vacuum suction boxes and vacuum rollers, and then dried by drying cylinders. The dryness of the paper sheets is controlled at 94% when they leave the drying cylinders.
[0068] (5) Crinkling and rolling: The dried paper sheet is wrinkled at a wrinkling scraper with a wrinkling rate of 24%. The wrinkled paper sheet is rolled up to obtain comparative household paper No. 1.
[0069] Comparative Example 2 Comparative Tissue Paper 2#
[0070] The preparation method comprises the following steps:
[0071] (1) Double disc mill low-concentration pulping was used, and the solvent-based cellulose was reed pulp prepared with an organic acid solvent, with a pulping concentration of 3.9% and a beating degree of 45°SR;
[0072] (2) Two-stage combined refining is used for coniferous chemical pulp, and double-disc low-concentration refining is used for broadleaf chemical pulp. The refining concentration of bleached coniferous chemical pulp is 3.59%, the beating degree is 27°SR, and the refining concentration of bleached broadleaf pulp is 3.26%, and the beating degree is 22°SR.
[0073] (3) Pulping: Pulping ratio: 70% solvent-processed reed pulp, 10% bleached coniferous chemical pulp, 20% bleached broadleaf chemical pulp, paper weight 16.4g / m 2 The wet strength agent is polyamide epichlorohydrin type, the addition amount is 2% of the total slurry absolute dry mass, the softener is quaternary ammonium salt type, the addition amount is 0.5% of the total slurry absolute dry mass, and the papermaking is carried out after mixing evenly;
[0074] (4) Dehydration and drying: The wet paper sheets are dehydrated in turn by vacuum suction boxes and vacuum rollers, and then dried by drying cylinders. The dryness of the paper sheets is controlled at 94% when they leave the drying cylinders.
[0075] (5) Crinkling and rolling: The dried paper sheet is wrinkled at a wrinkling scraper with a wrinkling rate of 23%. The wrinkled paper sheet is rolled up to obtain comparative household paper 2#.
[0076] Comparative Example 3: Comparison of tissue paper #3
[0077] (1) using a high-consistency refiner for refining, the solvent-based cellulose is a reed pulp prepared from an organic alcohol solvent, the refining concentration is 20%, and the beating degree is 41°SR;
[0078] (2) The coniferous chemical pulp adopts two-stage combined refining, the bleached coniferous chemical pulp refining concentration is 3.38%, and the beating degree is 27°SR;
[0079] (3) Pulping: 70% solvent-processed reed pulp, 30% bleached coniferous chemical pulp, paper weight 16.1g / m 2 The wet strength agent is polyamide epichlorohydrin, the addition amount is 1% of the absolute dry weight of the total slurry, no softener is added, and papermaking is carried out after mixing evenly;
[0080] (4) Dehydration and drying: The wet paper sheets are dehydrated by vacuum suction boxes and vacuum rollers, and then dried by drying cylinders. The dryness of the paper sheets is controlled at 92% when they leave the drying cylinders.
[0081] (5) Crinkling and rolling: The dried paper sheet is wrinkled at a wrinkling scraper with a wrinkling rate of 27%. The wrinkled paper sheet is rolled up to obtain comparative household paper #3.
[0082] Comparative Example 4 vs. Living Paper 4#
[0083] (1) using a high-consistency refiner for pulping, the solvent-based cellulose is reed pulp prepared with an organic acid solvent, the pulping concentration is 19%, and the beating degree is 43°SR;
[0084] (2) The coniferous chemical pulp adopts two-stage combined refining, the bleached coniferous chemical pulp refining concentration is 3.61%, and the beating degree is 26°SR;
[0085] (3) Pulping: 50% solvent-processed reed pulp, 50% bleached coniferous chemical pulp, paper weight 16.5g / m 2 The wet strength agent is polyamide epichlorohydrin, the addition amount is 1.5% of the total dry mass of the slurry, the softener is quaternary ammonium salt type, the addition amount is 0.5% of the total dry mass of the slurry, and the papermaking is carried out after mixing evenly;
[0086] (4) Dehydration and drying: The wet paper sheets are dehydrated in a vacuum suction box and vacuum rollers, and then dried by a drying cylinder. The dryness of the paper sheets is controlled at 93% when they leave the drying cylinder.
[0087] (5) Crinkling and rolling: The dried paper sheet is wrinkled at a wrinkling scraper with a wrinkling rate of 28%. The wrinkled paper sheet is rolled up to obtain comparative household paper 4#.
[0088] Experimental example
[0089] 1. Performance Testing
[0090] The performance indicators of the paper sheets produced in the above embodiments and comparative examples were tested in accordance with GB T20810-2018, wherein the larger the tensile index and wet strength values, the higher the strength performance of the paper sheets, the smaller the softness value, the softer the paper sheets, and the larger the bulk value, the fluffier the paper sheets, and the better the actual hand feel experience.
[0091] The test results are shown in Table 1.
[0092] Table 1 Performance test
[0093]
[0094]
[0095] From the above data, it can be seen that the dry tensile strength of the paper prepared by the method defined in this application is basically the same as that of the mainstream brands on the market, but the bulk is significantly improved, which will bring a fluffier feel and effectively improve the actual use experience of the product. At the same time, the paper prepared in this application has high wet strength and is not easy to break.
[0096] Comparative Example 1 is a solvent-based straw pulp using conventional low-concentration pulping, and Comparative Example 2 is a solvent-based straw pulp and bleached broadleaf pulp using conventional low-concentration pulping. From the perspective of paper performance indicators, the dry and wet strengths are reduced to a certain extent, and the bulk is poor. The reason is analyzed as the use of low-concentration pulping makes the metal grinding disc contact the fiber directly, and its cutting effect is strong. The straw pulp and broadleaf wood pulp fibers are short, and low-concentration pulping will cause the average fiber length to decrease. Therefore, the bulk and strength of the paper are reduced to a certain extent, and the softness increases; in Comparative Example 3, the proportion of coniferous chemical pulp exceeds the range specified in this application. The results show that its strength is improved, but the softness and bulk are poor; in Comparative Example 4, the proportion of solvent-based cellulose pulp is smaller than the range specified in this application. Although the strength is improved, due to the excessively high proportion of bleached coniferous pulp, the paper has a high hardness and poor hand feel.
[0097] 2. Metal ion content test
[0098] The household paper No. 1 prepared in Example 1 was tested against a certain brand of straw pulp household paper on the market. The results are shown in Table 2.
[0099] Table 2 Determination of metal ion content
[0100]
[0101] It can be seen from the data in the above table that the paper prepared in Example 1 does not contain any heavy metal ions, and the contents of other metal ions are significantly lower than those of conventional straw pulp products. The reason for this is that the solvent-based cellulose is used, so that most of the metal ions in the pulp are dissolved in the organic solvent, and thus are taken away and do not remain in the pulp, and thus will not remain in the final finished paper, thereby bringing safer and more reliable household paper products.
[0102] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing solvent-processed plant fiber household paper, It is characterized in that The following steps are involved: (1) Solvent-based cellulose pretreatment: Refining is performed using a high-consistency refiner. Solvent-based cellulose is prepared using any solvent including organic acids, alcohols or esters; (2) Pretreatment of coniferous and broadleaf chemical pulp: coniferous chemical pulp is refined by two-stage combined pulping, and broadleaf chemical pulp is refined by a high-consistency refiner; (3) pulping: according to weight percentage, the coniferous chemical pulp is 10-20%, the broadleaf chemical pulp is 0-20%, and the solvent-based cellulose is 70-90%. After the pulping is completed, a wet strength agent or a combination of a wet strength agent and a softener is added, and the mixture is evenly mixed before papermaking; (4) Dehydration and drying: The wet paper sheets made by the papermaking machine are dehydrated and then dried; (5) wrinkling and rolling: the dried paper sheet is wrinkled at a wrinkling scraper, and the wrinkled paper sheet is rolled up to obtain the solvent-processed plant fiber household paper; Wherein, in step (1), the pulping concentration is 15-25%, and the pulp beating degree is controlled to be 35-45°SR; The preparation method of solvent-based cellulose comprises the following steps: mixing wood chips, bamboo chips and straw, steaming them at 50-200°C for 30-120 minutes with an alcohol or organic acid or ester aqueous solution, washing the pulp and performing single-stage or multi-stage combined bleaching with a bleaching agent to obtain the cellulose.
2. The preparation method according to claim 1, It is characterized in that In step (2), the pulping concentration of coniferous chemical pulp is 3-4%, and the pulping beating degree is controlled at 25-35°SR; the pulping concentration of broadleaf chemical pulp is 15-25%, and the pulping beating degree is controlled at 20-30°SR.
3. The preparation method according to claim 1, It is characterized in that In step (3), the amount of wet strength agent added is 1-10% of the absolute dry mass of the total slurry, the amount of softener added is 0-1.5% of the absolute dry mass of the total slurry, and the basis weight of the paper sheet is 10-20 g / m 2 .
4. The preparation method according to claim 3, It is characterized in that The wet strength agent is any one of polyamide epichlorohydrin, urea-formaldehyde resin, dialdehyde starch, and glyoxal polyamide resin.
5. The preparation method according to claim 3, It is characterized in that The softener is any one of quaternary ammonium salt type, silicone type, water-based polyurethane, and polyethylene type.
6. The preparation method according to claim 1, It is characterized in that In step (4), the wet paper sheets are dehydrated in turn by a vacuum water suction box and a vacuum roller, and then dried by a drying cylinder. The dryness of the paper sheets is controlled at 88%-95% when they leave the drying cylinder.
7. The preparation method according to claim 1, It is characterized in that In step (5), the wrinkling rate is controlled at 20-30%.
8. A solvent-processed plant fiber tissue paper, It is characterized in that Prepared by any one of the methods of claims 1-7.