A black phosphorus modified composite diaphragm for aqueous zinc ion battery and its preparation method and application
The black phosphorus modified composite separator forms a zinc phosphate protective layer in the aqueous zinc ion battery, which solves the problems of zinc negative electrode corrosion and dendrite growth, extends the battery's short-circuit time and improves the cycle life and capacity of the entire battery, and achieves more High battery performance and stability.
Patent Information
- Application Number
- CN202310497121.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-05-05
AI Technical Summary
The zinc negative electrode in zinc ion batteries is prone to corrosion, dendrite growth and interface passivation problems, resulting in limited cycle stability, and existing diaphragms are difficult to effectively suppress, affecting battery performance and safety.
The preparation method of black phosphorus modified composite separator is adopted to form a black phosphorus dispersion by ultrasonic peeling, and the battery separator is placed in it. After drying, the black phosphorus modified composite separator is obtained, which is used in aqueous zinc ion batteries to form a zinc phosphate protective layer. To inhibit zinc dendrites growth and hydrogen evolution activity.
Significantly extend the short circuit time of zinc-zinc symmetrical batteries, improve the cycle life and capacity of zinc-hydrated vanadium pentoxide full battery, and improve the cycle stability and battery performance of zinc negative electrodes.
Smart Images

Figure CN116598703B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of zinc ion batteries, and in particular to a black phosphorus modified composite diaphragm for aqueous zinc ion batteries, and a preparation method and application thereof. Background Art
[0002] The widely used lithium-ion batteries based on liquid organic electrolytes have great safety risks due to the high flammability of organic liquids, which has been verified in many lithium-ion battery energy storage power station combustion / explosion accidents at home and abroad. Therefore, there is an urgent need to develop safer and more reliable electrochemical energy storage systems.
[0003] Metal batteries based on aqueous electrolytes show great advantages in this regard due to the intrinsic safety characteristics of aqueous electrolytes. Traditional alkaline metal batteries (such as Li, Na and K) react violently with water, which can lead to serious side reactions. Therefore, researchers have paid more attention to aqueous multivalent metal batteries (such as Ca, Mg, Al, Mn, Zn and Fe) in recent years. Among them, Zn metal can achieve a balance between the hydrogen evolution side reaction and the full battery voltage output platform due to its moderate potential for hydrogen. In addition, Zn metal as a negative electrode has a theoretical mass specific capacity (820mAh g -1 ) and volumetric capacity (5855 mAh cm -3 ) high, strong deposition / dissolution kinetics, abundant reserves, low cost, and environmental friendliness, it stands out among many metal anodes and has attracted much attention in recent years.
[0004] However, the current zinc metal battery has not yet achieved large-scale commercialization, mainly because the zinc negative electrode side is widely subject to scientific problems such as corrosion, hydrogen evolution, dendrite growth, and interface passivation, which results in limited negative electrode cycle stability. CN114725537A discloses an aqueous zinc ion battery electrolyte and its application that can inhibit zinc dendrites and side reactions. From the perspective of electrolyte modification, the electrolyte includes zinc sulfate, deionized water, and organic additives tripropylene glycol and propylene glycol. By changing the volume of tripropylene glycol and propylene glycol additives, mixed electrolytes with different volume ratios are obtained. The use of an electrolyte containing tripropylene glycol and propylene glycol additives can effectively improve the reversibility of the metal zinc negative electrode, reduce the occurrence of battery side reactions, and obtain an aqueous zinc ion battery with long life, excellent performance, and high safety.
[0005] CN114824236A discloses an aqueous zinc ion battery negative electrode material with a functional protective layer and a preparation method thereof. The preparation method uses a zinc sheet as a substrate, and mixes zinc sulfate heptahydrate, sodium phosphite, stannous chloride dihydrate, boric acid, sodium sulfate, disodium ethylenediaminetetraacetic acid and deionized water to form an electroplating solution, and uses an electrodeposition method to uniformly deposit tin-doped zinc phosphide on the zinc sheet to form a coating (Zn@Sn-ZnP). The invention constructs a Sn-ZnP functional protective layer on the surface of the metal zinc negative electrode, and inserts P into the Zn lattice to form a ZnP protective layer through an economical and efficient electrodeposition method, which is beneficial to Zn 2+ The ZnSn alloy formed by electrodeposition can effectively inhibit the hydrogen evolution reaction and the formation of irreversible byproducts of the zinc electrode, thereby improving the cycle life of the battery. However, the protective effect of the above method is not long-lasting, the effect of improving battery performance is limited, or there is a problem that the preparation method of the zinc sheet electrode is relatively complicated.
[0006] The separators (such as glass fiber) widely used in zinc-ion batteries can only provide the function of isolating the positive and negative electrodes, and it is difficult to have a suppressive effect on these scientific problems of the negative electrode. Therefore, it is of great significance to further study the separator materials that can improve the above scientific problems, especially play a sustained role. Summary of the invention
[0007] The present invention aims to solve the problems of easy corrosion, dendrite growth and interface passivation of the zinc negative electrode in aqueous zinc ion batteries, and provides a composite diaphragm that can continuously improve the stripping / deposition stability of the zinc negative electrode and a preparation method thereof. The diaphragm can achieve a long-term, stable and continuous improvement effect, thereby improving the cycle stability of the zinc negative electrode.
[0008] To achieve the above object, the technical solution adopted by the present invention is:
[0009] A method for preparing a black phosphorus modified composite diaphragm for an aqueous zinc ion battery comprises the steps of placing black phosphorus in a solution for ultrasonic stripping to obtain a black phosphorus dispersion, placing a battery diaphragm in the black phosphorus dispersion for ultrasonic stripping, taking out the battery diaphragm and drying it to obtain the black phosphorus modified composite diaphragm.
[0010] In some embodiments, the black phosphorus ultrasonic exfoliation time is more than 30 minutes. The black phosphorus block is effectively exfoliated by ultrasonic exfoliation to form a uniformly dispersed black phosphorus dispersion.
[0011] In some embodiments, the battery separator is ultrasonically treated in the black phosphorus dispersion for 15-30 minutes. Too long a time may easily cause the separator substrate structure to be damaged, such as 20 minutes, 25 minutes, or any value therebetween.
[0012] In some embodiments, the solution includes a mixed solution of one or more of water, ethanol, NMP, IPA, DMF, and DMSO; any common polar solvent can be used, which can effectively disperse the black phosphorus solid.
[0013] In some embodiments, the battery separator includes a composite membrane of any one or more of a glass fiber membrane, a polyolefin membrane, a cellulose membrane, and a Nafion membrane, preferably a glass fiber membrane, which has excellent electrolyte wettability.
[0014] In some embodiments, the mass concentration of black phosphorus in the black phosphorus dispersion is 5-20 mg mL -1 The loading amount of black phosphorus in the black phosphorus modified composite membrane is 0.6-2.5 mg cm -2 The zinc phosphate protective layer formed by hydrolysis under this condition has moderate thickness. After being applied to the battery, the battery performance is excellent, and the short-circuit time of the short-circuit battery can exceed 1500 hours.
[0015] In some embodiments, the mass concentration of black phosphorus in the black phosphorus dispersion is 5-15 mg mL -1 The loading amount of black phosphorus in the black phosphorus modified composite membrane is 1.5-2.5 mg cm -2 .
[0016] In some embodiments, the drying condition is 50-80° C. for 6-18 h.
[0017] The present invention also provides a black phosphorus modified composite diaphragm prepared according to the preparation method and the application of the black phosphorus modified composite diaphragm in an aqueous zinc ion battery, including application in a zinc-zinc symmetrical battery or a zinc-hydrated vanadium pentoxide full battery. When applied to a zinc-zinc symmetrical battery, the short circuit time of the battery is significantly prolonged.
[0018] The present invention also provides a zinc-hydrated vanadium pentoxide full battery, which uses the black phosphorus modified composite diaphragm as the battery diaphragm, a zinc salt aqueous solution as the electrolyte, a zinc foil as the negative electrode and the counter electrode, and hydrated vanadium pentoxide as the positive electrode, and the cycle life and capacity of the full battery are significantly improved.
[0019] In some embodiments, the zinc salt includes any one or more of ZnSO4, Zn(TFSI)2, Zn(TfO)2, etc. In some embodiments, the molar concentration of the zinc salt in the aqueous electrolyte is 2-3 mol L -1 If the concentration is too low, there will be too much unsolvated water in the electrolyte, causing the hydrolysis to be too fast; if the concentration is too high, there will be too little unsolvated water in the electrolyte, causing the hydrolysis to be too slow.
[0020] In some embodiments, the process for preparing a hydrated vanadium pentoxide positive electrode comprises: adding V2O5 powder and H2O2 to deionized water. After aging, the obtained hydrated vanadium pentoxide precipitate is collected, washed and freeze-dried.
[0021] The hydrated vanadium pentoxide powder is mixed with polyvinylidene fluoride (PVDF). The mixture is then dispersed in NMP solvent. The mixed slurry is coated on carbon paper and dried in a vacuum oven to obtain a hydrated vanadium pentoxide positive electrode.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] In the present invention, black phosphorus is used to modify the battery separator. The black phosphorus in the modified composite separator will gradually react and hydrolyze with water in the aqueous electrolyte and form a zinc phosphate interface layer with the zinc surface, thereby inhibiting the growth of zinc dendrites, inhibiting hydrogen evolution activity, and improving the cycle life of the zinc negative electrode. Compared with strategies such as (i) unmodified separator, (ii) unmodified separator + zinc negative electrode surface zinc phosphate pre-construction, (iii) unmodified separator + electrolyte phosphoric acid pre-addition, the black phosphorus modified separator of the present invention can achieve better zinc metal stripping / deposition stability, which is manifested in the extension of the short-circuit time of the zinc-zinc symmetric battery, and at the same time, the cycle life and capacity of the zinc-hydrated vanadium pentoxide full battery are greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a physical picture of the black phosphorus modified glass fiber membrane #1 in Example 1.
[0025] Figure 2 The scanning electron microscope image and element distribution map of the black phosphorus modified glass fiber membrane #1 in Example 1.
[0026] Figure 3 Voltage-time curve of zinc-zinc symmetric cell assembled with black phosphorus modified glass fiber separator #1 in Example 1
[0027] Figure 4 This is the cycling performance diagram of the zinc-hydrated vanadium pentoxide full battery assembled with black phosphorus modified glass fiber separator #1 in Example 1.
[0028] Figure 5 This is a physical picture of the glass fiber diaphragm of comparative example 1.
[0029] Figure 6 This is a scanning electron microscope image of the glass fiber diaphragm of Comparative Example 1.
[0030] Figure 7 This is the voltage-time curve of the zinc-zinc symmetric battery assembled with glass fiber separator in comparative example 1.
[0031] Figure 8This is the distribution diagram of zinc phosphate on the surface of the zinc negative electrode after immersion in phosphoric acid in Comparative Example 2, a is a three-dimensional perspective view of PO4 negative ions on the surface of the zinc sheet, and b is the corresponding side view.
[0032] Fig. 9 This is the voltage-time curve of the zinc-zinc symmetric battery assembled with glass fiber separator in comparative example 2.
[0033] Fig.10 This is the voltage-time curve of the zinc-zinc symmetric battery assembled with glass fiber diaphragm in comparative example 3.
[0034] Fig.11 This is a scanning electron microscope image of the zinc negative electrode surface of the symmetrical battery in Example 1 after 100 hours of cycling.
[0035] Fig.12 This is a scanning electron microscope image of the zinc negative electrode surface of the symmetrical battery in Comparative Example 1 after 100 hours of cycling.
[0036] Fig.13 These are scanning electron microscope images of the zinc negative electrode morphology of the symmetrical batteries in Example 1 and Comparative Examples 2-3 after 300 hours of cycling, (a) Example 1, (b) Comparative Example 2, and (c) Comparative Example 3.
[0037] Fig.14 These are scanning electron microscope images of the zinc negative electrode cross-sections of the symmetrical batteries in Example 1 and Comparative Examples 2-3 after 300 hours of cycling, (a) Example 1, (b) Comparative Example 2, and (c) Comparative Example 3.
[0038] Fig.15 This is a test graph of ionic conductivity during the hydrolysis of black phosphorus in 2M zinc sulfate electrolyte in Example 4. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art can make modifications or equivalent substitutions based on the understanding of the technical scheme of the present invention without departing from the spirit and scope of the technical scheme of the present invention, and all should be included in the protection scope of the present invention.
[0040] The raw materials used in the following specific embodiments are all purchased from the market.
[0041] The calculation method of the black phosphorus loading on the diaphragm is as follows: weigh the untreated battery diaphragm with a diameter of 14 mm as m0, sonicate the battery diaphragm in the black phosphorus dispersion, take it out and dry it, then weigh it as m1, and the black phosphorus loading on the modified composite diaphragm is m1-m0 / area.
[0042] Example 1
[0043] Preparation of black phosphorus modified glass fiber separator #1 and its application in aqueous zinc batteries
[0044] The black phosphorus block was placed in NMP solvent and ultrasonically exfoliated for 30 min to obtain a mass concentration of 10 mg mL -1 A commercial glass fiber (GF / A model, 14 mm in diameter) diaphragm was placed in the dispersion and ultrasonicated for 30 minutes. The diaphragm was taken out and dried in a vacuum drying oven at 60°C for 12 hours to obtain diaphragm #1. The actual picture is as follows Figure 1 As shown. The black phosphorus loading is 1.78 mg / cm 2 , scanning electron microscope and X-ray spectrum diagram as shown Figure 2 As shown, it is proved that black phosphorus is evenly distributed on the separator fibers.
[0045] Vanadium pentoxide powder (3.64 g) and 30% hydrogen peroxide (16 mL) were added to 200 mL of deionized water. After 24 hours of aging, the hydrated vanadium pentoxide precipitate was collected, washed and freeze-dried for 12 hours. The hydrated vanadium pentoxide powder was mixed with polyvinylidene fluoride (PVDF) in a mass ratio of 9:1. The mixture was then dispersed in NMP solvent. The mixed slurry was coated on carbon paper and dried at 60°C in a vacuum oven for 12 hours to obtain a hydrated vanadium pentoxide positive electrode.
[0046] Application of diaphragm
[0047] 1. Zinc-zinc symmetrical battery
[0048] The obtained composite membrane was used as a zinc ion battery membrane, 2 mol L -1 The ZnSO4 aqueous solution was used as the electrolyte; the zinc foil was used as the negative electrode and the zinc foil as the counter electrode to assemble the button cell and perform constant current charge and discharge tests with a current density of 5 mA cm -2 , with a cut-off capacity of 1 mA cm -2 Its voltage-time curve is as follows Figure 3 As shown, after 3500 hours of cycling, the battery still did not show short circuit phenomenon, and the short circuit time exceeded 3500 hours.
[0049] 2. Zinc-hydrated vanadium pentoxide full battery
[0050] The obtained composite membrane was used as a zinc ion battery membrane, 2 mol L -1 The ZnSO4 aqueous solution was used as the electrolyte; zinc foil was used as the negative electrode and hydrated vanadium pentoxide was used as the positive electrode to assemble a button cell and perform constant current charge and discharge tests with a current density of 2A g -1 (Based on the mass of hydrated vanadium pentoxide), the voltage range is 0.6-1.6V. Cyclic performance is as follows Figure 4As shown, the battery’s first discharge capacity is 203 mAh g -1 , the capacity retention rate is 90% after 1500 cycles.
[0051] Example 2
[0052] Preparation of black phosphorus modified glass fiber separator #2 and its application in aqueous zinc batteries
[0053] The black phosphorus block was placed in NMP solvent and ultrasonically exfoliated for 30 min to obtain a mass concentration of 5 mg mL -1 A commercial glass fiber (GF / A model, 14 mm in diameter) diaphragm was placed in the dispersion and ultrasonicated for 30 minutes. The obtained diaphragm was placed in a vacuum drying oven and dried at 60°C for 12 hours to obtain diaphragm #2. The black phosphorus loading was 0.76 mg / cm 2 .
[0054] Vanadium pentoxide powder (3.64 g) and 30% hydrogen peroxide (16 mL) were added to 200 mL of deionized water. After 24 hours of aging, the hydrated vanadium pentoxide precipitate was collected, washed and freeze-dried for 12 hours. The hydrated vanadium pentoxide powder was mixed with polyvinylidene fluoride (PVDF) in a mass ratio of 9:1. The mixture was then dispersed in NMP solvent. The mixed slurry was coated on carbon paper and dried at 60°C in a vacuum oven for 12 hours to obtain a hydrated vanadium pentoxide positive electrode.
[0055] Application Process:
[0056] 1. Zinc-zinc symmetrical battery
[0057] The obtained composite membrane was used as a zinc ion battery membrane, 2 mol L -1 The ZnSO4 aqueous solution was used as the electrolyte; the zinc foil was used as the negative electrode and the zinc foil as the counter electrode to assemble the button cell and perform constant current charge and discharge tests with a current density of 5 mA cm -2 , with a cut-off capacity of 1 mA cm -2 The short-circuit time is 1534 hours, which is lower than that of Example 1.
[0058] 2. Zinc-hydrated vanadium pentoxide full battery
[0059] The obtained composite membrane was used as a zinc ion battery membrane, 2 mol L -1 The ZnSO4 aqueous solution was used as the electrolyte; zinc foil was used as the negative electrode and hydrated vanadium pentoxide was used as the positive electrode to assemble a button cell and perform constant current charge and discharge tests with a current density of 2A g -1 (Based on the mass of hydrated vanadium pentoxide), the voltage range is 0.6-1.6V. The first discharge capacity of the battery is 192mAhg-1 , the capacity retention rate after 1500 cycles is 81%, which is slightly lower than that of Example 1 due to the low black phosphorus loading.
[0060] Example 3
[0061] Preparation of black phosphorus modified glass fiber separator #3 and its application in aqueous zinc batteries
[0062] The black phosphorus block was placed in NMP solvent and ultrasonically exfoliated for 30 min to obtain a mass concentration of 10 mg mL -1 A commercial glass fiber (GF / A model, 14 mm in diameter) diaphragm was placed in the dispersion and ultrasonicated for 30 minutes. The obtained diaphragm was placed in a vacuum drying oven and dried at 60°C for 12 hours to obtain diaphragm #1, with a black phosphorus loading of 1.78 mg / cm 2 .
[0063] Vanadium pentoxide powder (3.64 g) and 30% hydrogen peroxide (16 mL) were added to 200 mL of deionized water. After 24 hours of aging, the hydrated vanadium pentoxide precipitate was collected, washed and freeze-dried for 12 hours. The hydrated vanadium pentoxide powder was mixed with polyvinylidene fluoride (PVDF) in a mass ratio of 9:1. The mixture was then dispersed in NMP solvent. The mixed slurry was coated on carbon paper and dried at 60°C in a vacuum oven for 12 hours to obtain a hydrated vanadium pentoxide positive electrode.
[0064] Application Process:
[0065] 1. Zinc-zinc symmetrical battery
[0066] The obtained composite membrane #1 was used as a zinc ion battery membrane, 5 mol L -1 The ZnSO4 aqueous solution was used as the electrolyte; the zinc foil was used as the negative electrode and the zinc foil as the counter electrode to assemble the button cell and perform constant current charge and discharge tests with a current density of 5 mA cm -2 , with a cut-off capacity of 1 mA cm -2 , and its short-circuit time is 2232 hours.
[0067] 2. Zinc-hydrated vanadium pentoxide full battery
[0068] The obtained composite membrane was used as a zinc ion battery membrane, 2 mol L -1 The ZnSO4 aqueous solution was used as the electrolyte; zinc foil was used as the negative electrode and hydrated vanadium pentoxide was used as the positive electrode to assemble a button cell and perform constant current charge and discharge tests with a current density of 2A g -1 (Based on the mass of hydrated vanadium pentoxide), the voltage range is 0.6-1.6V. The first discharge capacity of the battery is 191mAhg -1, the capacity retention rate is 77% after 1500 cycles.
[0069] Comparative Example 1
[0070] Preparation of unmodified glass fiber separator and its application in aqueous zinc batteries
[0071] Vanadium pentoxide powder (3.64 g) and 30% hydrogen peroxide (16 mL) were added to 200 mL of deionized water. After 24 hours of aging, the hydrated vanadium pentoxide precipitate was collected, washed and freeze-dried for 12 hours. The hydrated vanadium pentoxide powder was mixed with polyvinylidene fluoride (PVDF) in a mass ratio of 9:1. The mixture was then dispersed in NMP solvent. The mixed slurry was coated on carbon paper and dried at 60°C in a vacuum oven for 12 hours to obtain a hydrated vanadium pentoxide positive electrode.
[0072] 1. Zinc-zinc symmetrical battery
[0073] Commercial glass fiber (GF / A model, 14 mm in diameter) is used as a zinc ion battery separator. Figure 5 As shown in the scanning electron microscope image Figure 6 As shown. 2mol L -1 The ZnSO4 aqueous solution was used as the electrolyte; the zinc foil was used as the negative electrode and the zinc foil as the counter electrode to assemble the button cell and perform constant current charge and discharge tests with a current density of 5 mA cm -2 , with a cut-off capacity of 1 mA cm -2 .like Figure 7 As shown, its short circuit time is 359 hours.
[0074] 2. Zinc-hydrated vanadium pentoxide full battery
[0075] Commercial glass fiber (GF / A model, 14 mm in diameter) was used as a separator for zinc ion batteries. -1 The ZnSO4 aqueous solution was used as the electrolyte; zinc foil was used as the negative electrode and hydrated vanadium pentoxide was used as the positive electrode to assemble a button cell and perform constant current charge and discharge tests with a current density of 2A g -1 (based on the mass of hydrated vanadium pentoxide), the voltage range is 0.6-1.6V. The first discharge capacity of the battery is 182mAh g -1 , the capacity retention rate is 49% after 1500 cycles.
[0076] Comparative Example 2
[0077] Preparation of unmodified glass fiber separator and its application in aqueous zinc batteries
[0078] Vanadium pentoxide powder (3.64 g) and 30% hydrogen peroxide (16 mL) were added to 200 mL of deionized water. After 24 hours of aging, the hydrated vanadium pentoxide precipitate was collected, washed and freeze-dried for 12 hours. The hydrated vanadium pentoxide powder was mixed with polyvinylidene fluoride (PVDF) in a mass ratio of 9:1. The mixture was then dispersed in NMP solvent. The mixed slurry was coated on carbon paper and dried at 60°C in a vacuum oven for 12 hours to obtain a hydrated vanadium pentoxide positive electrode.
[0079] The zinc metal sheet was immersed in a 20 mM H3PO4 aqueous solution for 2 hours to obtain a zinc sheet rich in zinc phosphate on the surface. The time-of-flight secondary ion mass spectrometry (TOF-SIMS) is shown in Figure 8 As shown in Figure 1, a is a three-dimensional perspective view of PO4 anions on the surface of the zinc sheet, and b is the corresponding side view.
[0080] 1. Zinc-zinc symmetrical battery
[0081] Commercial glass fiber (GF / A model, 14 mm in diameter) was used as a separator for zinc ion batteries. -1 The ZnSO4 aqueous solution was used as the electrolyte; the above zinc sheet was used as the negative electrode, and the above zinc sheet was used as the counter electrode to assemble a button cell and perform a constant current charge and discharge test with a current density of 5 mA cm -2 , with a cut-off capacity of 1 mA cm -2 ,like Fig. 9 As shown, its short circuit time is 744 hours.
[0082] 2. Zinc-hydrated vanadium pentoxide full battery
[0083] Commercial glass fiber (GF / A model, 14 mm in diameter) was used as a separator for zinc ion batteries. -1 The ZnSO4 aqueous solution was used as the electrolyte; the above zinc sheet was used as the negative electrode and the hydrated vanadium pentoxide was used as the positive electrode to assemble a button cell and perform a constant current charge and discharge test with a current density of 2A g -1 (based on the mass of hydrated vanadium pentoxide), the voltage range is 0.6-1.6V. The first discharge capacity of the battery is 185mAh g -1 , the capacity retention rate is 71% after 1500 cycles.
[0084] Comparative Example 3
[0085] Preparation of unmodified glass fiber separator and its application in aqueous zinc batteries
[0086] Vanadium pentoxide powder (3.64 g) and 30% hydrogen peroxide (16 mL) were added to 200 mL of deionized water. After 24 hours of aging, the hydrated vanadium pentoxide precipitate was collected, washed and freeze-dried for 12 hours. The hydrated vanadium pentoxide powder was mixed with polyvinylidene fluoride (PVDF) in a mass ratio of 9:1. The mixture was then dispersed in NMP solvent. The mixed slurry was coated on carbon paper and dried at 60°C in a vacuum oven for 12 hours to obtain a hydrated vanadium pentoxide positive electrode.
[0087] 1. Zinc-zinc symmetrical battery
[0088] Commercial glass fiber (GF / A model, 14 mm in diameter) was used as a separator for zinc ion batteries. -1 The ZnSO4+20mM H3PO4 aqueous solution was used as the electrolyte; zinc foil was used as the negative electrode and zinc foil as the counter electrode to assemble the button battery and perform constant current charge and discharge tests with a current density of 5mA cm -2 , with a cut-off capacity of 1 mA cm -2 ,like Fig.10 As shown in the figure, the short circuit time is 768 hours. It can be seen that directly adding phosphoric acid to the electrolyte does not play an effective role.
[0089] 2. Zinc-hydrated vanadium pentoxide full battery
[0090] Commercial glass fiber (GF / A model, 14 mm in diameter) was used as a separator for zinc ion batteries. -1 The ZnSO4+20mM H3PO4 aqueous solution was used as the electrolyte; zinc foil was used as the negative electrode and hydrated vanadium pentoxide was used as the positive electrode to assemble the button battery and perform constant current charge and discharge tests with a current density of 2A. -1 (based on the mass of hydrated vanadium pentoxide), the voltage range is 0.6-1.6V. The first discharge capacity of the battery is 187mAh g -1 , the capacity retention rate is 74% after 1500 cycles.
[0091] Observation of zinc negative electrode morphology after application
[0092] The zinc negative electrode of the symmetrical battery in Example 1 and Comparative Example 1 after 100 hours of cycling was observed for surface morphology. Fig.11 and Fig.12 As shown, it can be seen that in Example 1, compared with Comparative Example 1, the surface dendrites of the zinc negative electrode after cycling are significantly reduced, which is also the reason for the prolonged short circuit time. This shows that the battery separator prepared by the present invention can effectively provide protection for the zinc negative electrode and inhibit the growth of dendrites when applied to zinc-zinc symmetrical batteries.
[0093] The morphology of the zinc negative electrode after the symmetrical battery in Example 1, Comparative Example 2 and Comparative Example 3 was observed after 300 hours of cycling. Fig.13 As shown, the cross section Fig.14 As shown, (a) Example 1, (b) Comparative Example 2, and (c) Comparative Example 3 indicate that compared with the initial zinc phosphate modification of the negative electrode in Comparative Example 2 and the introduction of phosphoric acid into the electrolyte in Comparative Example 3, the surface dendrites of the zinc negative electrode after cycling are significantly reduced, indicating the effectiveness of this strategy.
[0094] Example 4
[0095] The black phosphorus block was placed in a 2M ZnSO4 aqueous solution for 20 days and 60 days to observe the hydrolysis of black phosphorus and test the ionic conductivity of the electrolyte. The results are as follows: Fig.15 As shown, black phosphorus can continuously hydrolyze to generate phosphate in 2M ZnSO4 aqueous solution. This also shows that after 20 or 60 days, the black phosphorus block can still continuously release phosphate ions, thereby improving the cycle stability of the zinc negative electrode.
Claims
1. A method for preparing a black phosphorus modified composite diaphragm for an aqueous zinc ion battery, characterized in that: The method comprises the steps of placing black phosphorus in a solution and ultrasonically exfoliating the black phosphorus to obtain a black phosphorus dispersion, placing a battery separator in the black phosphorus dispersion and ultrasonically exfoliating the battery separator, taking out the battery separator and drying the separator to obtain the black phosphorus modified composite separator; The ultrasonic peeling time of black phosphorus is more than 30 minutes; The battery separator is ultrasonically treated in the black phosphorus dispersion for 15-30 min; the mass concentration of black phosphorus in the black phosphorus dispersion is 5-20 mg mL -1 ; The loading amount of black phosphorus in the black phosphorus modified composite membrane is 0.6-2.5 mg cm -2 .
2. The method for preparing a black phosphorus modified composite diaphragm for an aqueous zinc ion battery according to claim 1, characterized in that: The solution includes a mixed solution of one or more of water, ethanol, NMP, IPA, DMF, and DMSO; And / or, the battery separator includes any one or more composite membranes of glass fiber membrane, polyolefin membrane, cellulose membrane, and Nafion membrane.
3. The method for preparing a black phosphorus modified composite diaphragm for an aqueous zinc ion battery according to claim 1, characterized in that: The drying conditions are 50-80°C for 6-18 hours.
4. A black phosphorus modified composite diaphragm prepared according to the preparation method according to any one of claims 1 to 3.
5. Use of the black phosphorus modified composite diaphragm according to claim 4 in aqueous zinc ion batteries.
6. A zinc-hydrated vanadium pentoxide full battery, characterized in that: The black phosphorus modified composite diaphragm according to claim 4 is used as a battery diaphragm, a zinc salt aqueous solution is used as an electrolyte, a zinc foil is used as a negative electrode and a counter electrode, and hydrated vanadium pentoxide is used as a positive electrode.
7. The zinc-hydrated vanadium pentoxide full battery according to claim 6, characterized in that: The molar concentration of zinc salt in the electrolyte is 2-3 mol L -1 .
Citation Information
Patent Citations
Water-based zinc ion battery electrolyte capable of inhibiting zinc dendrites and side reactions and application of water-based zinc ion battery electrolyte
CN114725537A
Diaphragm for water-based zinc ion battery and preparation method of diaphragm