A microwave dielectric ceramic and its preparation method and application
By combining the mixed system of MgNb2O6, MgTiO3 and Ca1-nSm2n/3O3 with MnCO3 and/or Al2O3 auxiliary materials, the problem of insufficient quality factor and temperature stability in high-frequency communication of traditional ceramic materials is solved, and the dielectric constant is achieved. Adjustable and high-quality factors to meet the needs of high-frequency communication devices.
Patent Information
- Application Number
- CN202310615403.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-05-29
AI Technical Summary
Traditional ceramic materials are difficult to achieve high quality factors, temperature stability and dielectric constant adjustable in high-frequency communication, and cannot meet the needs of high-frequency communication devices.
By using a mixing system of MgNb2O6, MgTiO3 with a negative temperature coefficient and Ca1-nSm2n/3O3 with a positive temperature coefficient as the main material, and adding MnCO3 and/or Al2O3 as the auxiliary material, the composition composite technology and the mixing rule of dielectric constant are used. The dielectric constant is adjustable in the range of 25-35, and combined with the parallel model of quality factors and the superposition effect of resonant frequency, a microwave dielectric ceramic with high quality factors and temperature stability is prepared.
It realizes adjustable dielectric constant in the range of 25-35, the quality factor is not less than 84600, and the temperature stability is good (τf < ±9ppm/℃), which meets the production needs of resonators and filters for high-frequency communications.
Smart Images

Figure BDA0004253641420000041
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ceramic materials, and more specifically, to a microwave dielectric ceramic and a preparation method and application thereof. Background Art
[0002] As microwave communication technology develops towards high frequencies (millimeter waves), such as 5G communication frequencies of 2-30GHz, ceramic resonators and filters used therein are required to have higher quality factors (Qf) and good temperature stability (near-zero resonant frequency temperature coefficient τf <±10ppm / ℃). In order to meet the miniaturization of devices and the design requirements of different device sizes, ceramics are also required to have a higher dielectric constant (K) and be adjustable over a wider range.
[0003] The traditional method of adjusting temperature stability is to compound two materials with positive temperature coefficient and negative temperature coefficient. However, after the two materials are compounded, it is difficult to achieve adjustable dielectric constant in a wide range, thus failing to meet the needs of different designs (such as the typical MgTiO3-CaTiO3 system with good temperature stability, whose dielectric constant is only slightly adjustable between 19-21). Therefore, it is urgent to develop a microwave dielectric ceramic material with high quality factor, temperature stability, and adjustable dielectric constant in a wide range. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a microwave dielectric ceramic and a preparation method and application thereof. The microwave dielectric ceramic provided by the present invention not only has a high quality factor (Qf not less than 84600, and can even reach 104500), good temperature stability (τf<±9ppm / ℃), but also has a dielectric constant that is adjustable in a wide range of 25-35.
[0005] A first aspect of the present invention provides a microwave dielectric ceramic.
[0006] Specifically, a microwave dielectric ceramic includes a main material and an auxiliary material, wherein the main material includes (1-xy)MgNb2O6-xMgTiO3-yCa 1-n Sm 2n / 3 O3, the auxiliary material includes MnCO3 and / or Al2O3; wherein x=0.01-0.1, y=0.01-0.2, n=0.1-1.
[0007] The present invention combines MgNb2O6 and MgTiO3 with negative temperature coefficient and ultra-high quality factor and CaO3 with positive temperature coefficient. 1-n Sm 2n / 3The mixed system of O3 is used as the main material of microwave dielectric ceramics. The different microwave dielectric properties of the three are utilized. Through the component composite technology: the mixing law of dielectric constant, the parallel model of quality factor and the superposition effect of resonant frequency, microwave dielectric ceramics with medium dielectric constant and high quality factor with stable temperature are obtained. The dielectric constant can be adjusted in a wide range (25-35), which can meet the production needs of resonators and filters for high-frequency communications.
[0008] Preferably, x = 0.03-0.06, y = 0.05-0.15, n = 0.3-0.5, x, y and n are all molar ratios.
[0009] More preferably, x=0.03-0.06, y=0.05-0.15, and n=0.35-0.45.
[0010] Preferably, the auxiliary material comprises 0.1-1wt% of MnCO3 and 0.05-0.5wt% of Al2O3 based on the total mass of the main material.
[0011] Further preferably, the auxiliary material comprises 0.2-0.5wt% of MnCO3 and 0.05-0.2wt% of Al2O3 based on the total mass of the main material.
[0012] Preferably, the raw materials for preparing the main material include the following components: MgNb2O6, MgTiO3 and Ca 1-n Sm 2n / 3 O3.
[0013] A second aspect of the present invention provides a method for preparing a microwave dielectric ceramic.
[0014] A method for preparing microwave dielectric ceramics comprises the following steps:
[0015] The main material and the auxiliary material are mixed, granulated, pressed and formed to obtain a ceramic green body, and then the microwave dielectric ceramic is obtained after debinding and sintering.
[0016] Preferably, after mixing the main ingredient and the auxiliary ingredient, a grinding step is also included.
[0017] Preferably, the granulation is performed by mixing the main material and the auxiliary material and then adding a binder to perform granulation.
[0018] Preferably, the binder is polyvinyl alcohol (PVA).
[0019] Preferably, the compression molding pressure is 160-300 MPa.
[0020] Preferably, the sintering temperature is 1400-1500° C., and the sintering time is 3-8 hours.
[0021] Preferably, the raw materials for preparing the main material include the following components: MgO, Nb2O5, TiO2, CaCO3 and Sm2O3.
[0022] Preferably, the method for preparing the main ingredient comprises the following steps:
[0023] (1) Take MgO, Nb2O5, TiO2, CaCO3 and Sm2O3 as raw materials, and prepare MgNb2O6, MgTiO3 and CaCO3 as raw materials respectively. 1-n Sm 2n / 3 O3, mixed in chemical formula, ground, dried and calcined to obtain MgNb2O6, MgTiO3 and Ca 1-n Sm 2n / 3 O3 three kinds of synthetic materials;
[0024] (2) The three synthetic materials obtained in step (1) are mixed according to (1-xy)MgNb2O6-xMgTiO3-yCa 1-n Sm 2n / 3 O3 (wherein x=0.03-0.06, y=0.05-0.15, all are molar ratios) are mixed in a chemical formula ratio to obtain the main material.
[0025] Preferably, in step (1), the grinding time is 12-24 hours.
[0026] Preferably, in step (1), calcining at 1200-1300°C for 3-7 hours to obtain MgNb2O6; calcining at 1100-1200°C for 2-6 hours to obtain MgTiO3; calcining at 1150-1250°C for 2-6 hours to obtain Ca 1-n Sm 2n / 3 O3.
[0027] A third aspect of the present invention provides an application of microwave dielectric ceramics.
[0028] The invention discloses an application of microwave dielectric ceramic in the field of microwave communication.
[0029] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0030] The microwave dielectric ceramic provided by the present invention comprises a main material and an auxiliary material, wherein the main material comprises (1-xy)MgNb2O6-xMgTiO3-yCa 1-n Sm 2n / 3 O3, the auxiliary materials include MnCO3 and / or Al2O3, wherein x=0.01-0.1, y=0.01-0.2, n=0.1-1. The main materials used in the present invention are MgNb2O6, MgTiO3 and Ca 1-n Sm 2n / 3The microwave dielectric ceramic provided by the present invention has a high quality factor (Qf not less than 84600, and can even reach 104500), good temperature stability (τf<±9ppm / ℃), and an adjustable dielectric constant (dielectric constant is 25-35) in a wide range. The microwave dielectric ceramic provided by the present invention can meet the production requirements of resonators and filters for high-frequency communication. DETAILED DESCRIPTION
[0031] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0032] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0033] Example 1
[0034] A microwave dielectric ceramic comprises a main material and an auxiliary material, wherein the main material comprises (1-xy)MgNb2O6-xMgTiO3-yCa 1-n Sm 2n / 3 O3, the auxiliary material includes 0.25wt% MnCO3 accounting for the total mass of the main material and 0.2wt% Al2O3 accounting for the total mass of the main material; wherein x=0.03, y=0.05, n=0.3.
[0035] The method for preparing the microwave dielectric ceramic comprises the following steps:
[0036] (1) MgO, Nb2O5, TiO2, CaCO3 and Sm2O3 were selected as raw materials, and MgNb2O6, MgTiO3 and CaCO3 were prepared respectively. 1-n Sm 2n / 3O3 (where n = 0.35-0.45) chemical formula after mixing, placed in a ball mill grinding 12-24 hours, mixed evenly;
[0037] (2) After drying, MgO and Nb2O5 are calcined at 1200°C for 6 hours to obtain MgNb2O6; MgO and TiO2 are calcined at 1150°C for 4 hours to obtain MgTiO3; CaCO3 and Sm2O3 are calcined at 1200°C for 3 hours to obtain Ca 1-n Sm 2n / 3 O3;
[0038] (3) MgNb2O6, MgTiO3 and Ca 1-n Sm2n / 3 O3 three kinds of synthetic materials, according to (1-xy)MgNb2O6-xMgTiO3-yCa 1-n Sm 2n / 3 O3 is mixed in a chemical formula ratio, and MnCO3 and Al2O3 are added, and the mixture is ground again in a ball mill to obtain a powder;
[0039] (4) adding 2% PVA of the total weight of the powder to granulate the powder, and then pressing and molding the powder at 260 MPa to obtain a ceramic green body;
[0040] (5) The ceramic green body is debonded and sintered at 1480° C. for 4 hours to obtain microwave dielectric ceramics.
[0041] Embodiment 2-6
[0042] Embodiments 2-6 provide microwave dielectric ceramics, which differ from Embodiment 1 in that the contents of x, y, n, MnCO3 and Al2O3 are different. See Table 1 for details.
[0043] Comparative Example 1
[0044] This comparative example provides a microwave dielectric ceramic, which differs from Example 1 in that Sm2O3 is replaced by Bi2O3.
[0045] Product effect testing
[0046] The microwave dielectric ceramics provided in the above embodiments were subjected to performance tests using the "GBT 5597-1999 Test Method for Microwave Complex Permittivity of Solid Dielectrics", and the test results are shown in the following table.
[0047] Table 1 Parameters and performance test results of various embodiments
[0048]
[0049] As can be seen from the above table, the dielectric constant (K) of the microwave dielectric ceramics prepared in Examples 1-6 of the present invention is adjustable between 25-35, with a near-zero resonant frequency temperature coefficient (τf<±10ppm / °C), and a high quality factor (Qf>80000). However, the dielectric constant K of Comparative Example 1 is 41.2, the quality factor Qf is 34400, and the resonant frequency temperature coefficient is +18ppm / °C, which cannot meet the application requirements of high-frequency microwave communication devices.
Claims
1. A microwave dielectric ceramic, characterized in that: It includes a main material and an auxiliary material, wherein the main material includes (1-xy)MgNb2O6-xMgTiO3-yCa 1-n Sm 2n / 3 O3, the auxiliary material includes MnCO3 and / or Al2O3; wherein x=0.01-0.1, y=0.01-0.2, n=0.1-1, and n is not 1.
2. The microwave dielectric ceramic according to claim 1, characterized in that: Said x=0.03-0.06, y=0.05-0.15, n=0.3-0.
5.
3. The microwave dielectric ceramic according to claim 1, characterized in that: The auxiliary material comprises 0.1-1wt% of MnCO3 and 0.05-0.5wt% of Al2O3, accounting for the total mass of the main material.
4. The method for preparing the microwave dielectric ceramic according to any one of claims 1 to 3, characterized in that: The steps include: The main material and the auxiliary material are mixed, granulated, pressed and formed to obtain a ceramic green body, and then the microwave dielectric ceramic is obtained after debinding and sintering.
5. The preparation method according to claim 4, characterized in that: The compression molding pressure is 160-300 MPa.
6. The preparation method according to claim 4, characterized in that: The sintering temperature is 1400-1500° C., and the sintering time is 3-8 hours.
7. The preparation method according to claim 4, characterized in that: The raw materials for preparing the main material include the following components: MgO, Nb2O5, TiO2, CaCO3 and Sm2O3.
8. The preparation method according to claim 7, characterized in that: The preparation method of the main material comprises the following steps: (1) Take MgO, Nb2O5, TiO2, CaCO3 and Sm2O3, respectively according to MgNb2O6, MgTiO3 and Ca 1-n Sm 2n / 3 O3, mixed in chemical formula, ground, dried and calcined to obtain MgNb2O6, MgTiO3 and Ca 1-n Sm 2n / 3 O3 three kinds of synthetic materials; (2) The three synthetic materials obtained in step (1) are mixed according to (1-xy)MgNb2O6-xMgTiO3-yCa 1-n Sm 2n / 3 O3 is mixed in the chemical formula ratio to obtain the main material.
9. The preparation method according to claim 8, characterized in that: In step (1), calcining at 1200-1300°C for 3-7 hours to obtain MgNb2O6; calcining at 1100-1200°C for 2-6 hours to obtain MgTiO3; calcining at 1150-1250°C for 2-6 hours to obtain Ca 1-n Sm 2n / 3 O3.
10. Application of the microwave dielectric ceramic according to any one of claims 1 to 3 in the field of microwave communication.