A dynamic strain aging strengthening process in the manufacturing process of non-quenched and tempered weathering bolts
By introducing two dynamic strain aging processes in the manufacturing process of non-quenched and tempered bolts, controlling the temperature, holding time and process parameters, the dislocation problem in the deformation structure is solved, the performance and production efficiency of the bolts are improved, and the cost is reduced.
Patent Information
- Application Number
- CN202310433975.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-04-21
AI Technical Summary
Non-quenched and tempered bolts have high-density movable dislocations and defects in the deformation structure during the production process, resulting in micro-yield. The existing aging treatment takes a long time and consumes a lot of energy, which increases the production cost.
Two dynamic strain aging processes are added to the manufacturing process of non-quenched and tempered bolts: in the first stage, the drawn bar is heated to 250°C~400°C and rolled, and in the second stage, the bolts after cold heading are heated to 150℃~300℃ and perform thread rolling. Control the temperature, holding time, pressing amount and speed of each process to stabilize dislocations and improve material utilization and performance.
It effectively prevents movable dislocation from climbing, improves the deformation strengthening performance of bolts, reduces aging processing time and energy consumption, reduces production costs, and meets the mechanical performance requirements of bolts of different specifications in GB/T 3098.1.
Abstract
Description
Technical Field
[0001] The invention relates to a dynamic strain aging strengthening process in a manufacturing process of a non-quenched and tempered weather-resistant bolt, and belongs to the technical field of steel for fasteners. Background Art
[0002] Non-quenched and tempered steel does not contain a large amount of alloy elements and does not require quenching and tempering treatment. It can save energy consumption in heat treatment and avoid waste caused by deformation or quenching cracks during heat treatment, and has been used more and more widely. However, the use of non-quenched and tempered steel to make bolts usually requires processes such as cold drawing, cold heading, and thread rolling. These processes will cause deformation structures in the bolts. There are high-density movable dislocations and other defects in this deformation structure, making it unstable. During the service of the bolts, these movable dislocations will climb and cause micro-yields. Aging treatment to stabilize movable dislocations can effectively prevent the occurrence of the above problems, but the aging treatment often takes a long time and consumes a lot of energy, which greatly increases the actual production cost. Therefore, it is necessary to develop a bolt production process that can save the above aging treatment and has good social and economic benefits. Summary of the invention
[0003] The purpose of the present invention is to solve the above-mentioned problems and provide a dynamic strain aging strengthening process in the manufacturing process of non-quenched and tempered weather-resistant bolts. The manufacturing process of the bolts in the present invention mainly includes: a drawing process, a first-stage dynamic strain aging process (rolling), a cold heading process, and a second-stage dynamic strain aging process (thread rolling), that is, two dynamic strain aging processes are added to the existing non-quenched and tempered bolt production process. In the drawing process in the process flow, the drawing reduction rate needs to be controlled at 10%~40% to make the deformation as small as possible. On the one hand, it can improve the utilization rate of materials, and on the other hand, it can avoid the generation of too many high-density areas of dislocation entanglement in the steel, so as to prepare for subsequent cold heading, rolling, thread rolling and other processes.
[0004] The technical scheme adopted by the present invention is: a dynamic strain aging strengthening process in the manufacturing process of non-quenched and tempered weather-resistant bolts, comprising the following steps: a drawing process, a first-stage dynamic strain aging process, a cold heading process, and a second-stage dynamic strain aging process, characterized in that in the first-stage dynamic strain aging process, the drawn bar is heated to 250°C~400°C and kept warm for 20min~40min; then rolling is immediately performed, and the rolling pressing amount is controlled to be 0.01mm~1.5mm; in the second-stage dynamic strain aging process, the bolts formed by cold heading are reheated to 150°C~300°C, kept warm for 10min~20min, and then the thread rolling process is immediately performed, and the thread rolling rate is controlled to be 10r / min~20r / min.
[0005] In the first stage of dynamic strain aging process, the heating temperature is controlled within the range of 250℃~400℃, the holding time is 20min~40min, and the rolling pressure is 0.01mm~1.5mm, so that the diffusion rate of solute atoms such as C and N in the steel at this temperature is equivalent to the dislocation movement rate generated by rolling, thereby stabilizing the movable dislocations generated by rolling and playing a significant deformation strengthening role. When the strain is low, there are only a small number of simple dislocation lines in the steel. As the strain increases, the number of dislocation lines increases, and dislocation entanglement begins to appear. At this time, only by increasing the heating temperature, so that the diffusion rate of solute atoms keeps up with the slip movement speed of dislocations, and a large enough Coriolis gas mass is formed to maintain the pinning effect on dislocations. These pinned dislocations can not only become dislocation sources for new dislocations, but also enable dislocation sources that cannot slip under low stress or dislocation sources of different slip systems to start when the external force increases the dislocations to get rid of the pinning, which ultimately leads to the continuous proliferation of dislocation sources and a significant increase in dislocation density. Therefore, the amount of rolling pressure must be determined in combination with the heating temperature during actual production.
[0006] In the second stage of dynamic strain aging process, the heating temperature is controlled at 150℃~300℃, the holding time is 10min~20min, and the rolling rate is 10r / min~20r / min. The strain amount of bolts with the same specifications during the rolling process is certain, and different rolling rates will result in different dislocation densities. Specifically, the dislocation density at a higher rolling rate is higher than that at a lower rolling rate. This is mainly because the bolts are rolled at a higher rolling rate, and the vacancies required for the diffusion of solute atoms are significantly increased, thereby shortening the time for the solute atoms to diffuse to the dislocations, making the interaction between the solute atoms and the dislocations significantly enhanced. At the same time, due to the reduction of the aging time, the number of dislocations recovered at high temperature is also significantly reduced. In addition, considering the influence of temperature on the diffusion rate of solute atoms and the influence of rolling rate on the movement speed of dislocations, the selection of the rolling rate should also be determined based on the actual heating temperature.
[0007] For bolts of the same specification, in the first stage dynamic strain aging process, the rolling pressure increases with the increase of temperature; in the second stage dynamic strain aging process, the thread rolling rate increases with the increase of temperature.
[0008] When processing bolts of different specifications, a certain margin must be reserved for the wire size after drawing, and the drawing reduction rate must be controlled between 10% and 40%. Implementation
[0009] Example
[0010] Processing method of M6 bolts: select non-quenched and tempered steel wire with a diameter of Φ6.8mm, draw it to Φ6.2mm, and the drawing reduction rate is 16.87%. Then carry out the first stage of dynamic strain aging: heat the drawn wire to 350℃, keep it warm for 25min, and then immediately roll it, control the rolling pressure to 0.21mm, and then carry out cold heading process to make the finished bolt. Finally, carry out the second stage of dynamic strain aging: reheat the physical bolt to 170℃, keep it warm for 15min, and then immediately roll it, and control the rolling rate to 15r / min. In this implementation case, the tensile strength of the M6 bolt is 850MPa and the yield strength is 780MPa, and its performance meets the mechanical property requirements of grade 8.8 bolts in GB / T 3098.1.
[0011] Example
[0012] Processing method of M10 bolts: select non-quenched and tempered steel wire with a diameter of Φ11.2mm, draw it to Φ9.8mm, and the drawing reduction rate is 23.43%. Then carry out the first stage of dynamic strain aging: heat the drawn wire to 250℃, keep it warm for 30min, and then immediately roll it, control the rolling pressure to 0.015mm, and then carry out cold heading process to make the finished bolt. Finally, carry out the second stage of dynamic strain aging: reheat the physical bolt to 200℃, keep it warm for 20min, and then immediately roll it, and control the rolling rate to 18r / min. In this implementation case, the tensile strength of the M10 bolt is 920MPa and the yield strength is 850MPa. Its performance meets the mechanical property requirements of 9.8 grade bolts in GB / T 3098.1.
[0013] Example
[0014] Processing method of M12 bolts: select non-quenched and tempered steel wire with a diameter of Φ14.2mm, draw it to Φ12.2mm, and the drawing reduction rate is 26.19%. Then carry out the first stage of dynamic strain aging: heat the drawn wire to 400℃, keep it warm for 35min, and then immediately roll it, control the rolling pressure to 0.25mm, and then carry out the cold heading process to make the finished bolt. Finally, carry out the second stage of dynamic strain aging: reheat the physical bolt to 260℃, keep it warm for 15min, and then immediately roll it, and control the rolling rate to 19r / min. In this implementation case, the tensile strength of the M12 bolt is 960MPa and the yield strength is 900MPa. Its performance meets the mechanical property requirements of grade 9.8 bolts in GB / T 3098.1.
[0015] Example
[0016] Processing method of M14 bolts: select non-quenched and tempered steel wire with a diameter of Φ16mm, draw it to Φ13.92mm, and the drawing reduction rate is 24.3%. Then carry out the first stage of dynamic strain aging: heat the drawn wire to 280℃, keep it warm for 25min, and then immediately roll it, control the rolling pressure to 0.06mm, and then carry out the cold heading process to make the finished bolt. Finally, carry out the second stage of dynamic strain aging: reheat the physical bolt to 150℃, keep it warm for 15min, and then immediately roll it, and control the rolling rate to 11r / min. In this implementation case, the tensile strength of the M12 bolt is 940MPa and the yield strength is 875MPa. Its performance meets the mechanical property requirements of grade 9.8 bolts in GB / T 3098.1.
Claims
1. A dynamic strain aging strengthening process in the manufacturing process of non-quenched and tempered weathering bolts, characterized in that: The method comprises the following steps: a drawing process, a first-stage dynamic strain aging process, a cold heading process, and a second-stage dynamic strain aging process. In the first-stage dynamic strain aging process, the drawn bar is heated to 250°C-400°C and kept warm for 20min-40min; then rolling is performed immediately, and the rolling pressure is controlled to be 0.01mm-1.5mm; in the second-stage dynamic strain aging process, the bolts formed by cold heading are reheated to 150°C-300°C and kept warm for 10min-20min, then the thread rolling process is performed immediately, and the thread rolling rate is controlled to be 10r / min-20r / min. For bolts of the same specification, in the first-stage dynamic strain aging process, the rolling pressure increases with the increase of temperature; in the second-stage dynamic strain aging process, the thread rolling rate increases with the increase of temperature.
2. The dynamic strain aging strengthening process in the manufacturing process of non-quenched and tempered weather-resistant bolts according to claim 1 is characterized in that: When processing bolts of different specifications, a certain margin must be reserved for the wire size after drawing, and the drawing reduction rate must be controlled between 10% and 40%.
3. The dynamic strain aging strengthening process in the manufacturing process of non-quenched and tempered weather-resistant bolts according to claim 1 is characterized in that: The method for processing M6 bolts is: The non-quenched and tempered steel wire with a diameter of Φ6.8mm is drawn to Φ6.2mm, and the drawing reduction rate is 16.87%; The first stage of dynamic strain aging is carried out: the drawn wire is heated to 350°C, kept warm for 25 minutes, and then rolled immediately, with the rolling pressure controlled to 0.21mm, and then cold heading is carried out to make the finished bolts; The second stage of dynamic strain aging is to reheat the physical bolts to 170°C, keep them warm for 15 minutes, and then immediately carry out thread rolling, controlling the thread rolling rate to 15r / min.
4. The dynamic strain aging strengthening process in the manufacturing process of non-quenched and tempered weather-resistant bolts according to claim 1 is characterized in that: The method for processing M10 bolts is: The non-quenched and tempered steel wire with a diameter of Φ11.2mm is drawn to Φ9.8mm, and the drawing reduction rate is 23.43%; The first stage of dynamic strain aging is carried out: the drawn wire is heated to 250°C, kept warm for 30 minutes, and then rolled immediately, with the rolling pressure controlled to 0.015mm, and then cold heading is carried out to make the finished bolts; The second stage of dynamic strain aging is to reheat the physical bolts to 200°C, keep them warm for 20 minutes, and then immediately carry out thread rolling, controlling the thread rolling rate to 18r / min.
5. The dynamic strain aging strengthening process in the manufacturing process of non-quenched and tempered weather-resistant bolts according to claim 1 is characterized in that: The method for processing M12 bolts is: The non-quenched and tempered steel wire with a diameter of Φ14.2mm is drawn to Φ12.2mm, and the drawing reduction rate is 26.19%; The first stage of dynamic strain aging is carried out: the drawn wire is heated to 400°C, kept warm for 35 minutes, and then rolled immediately, with the rolling pressure controlled to 0.25mm, and then cold heading is carried out to make the finished bolts; The second stage of dynamic strain aging is to reheat the physical bolts to 260°C, keep them warm for 15 minutes, and then immediately carry out thread rolling, controlling the thread rolling rate to 19r / min.
6. The dynamic strain aging strengthening process in the manufacturing process of non-quenched and tempered weather-resistant bolts according to claim 1 is characterized in that: The method for processing M14 bolts is: The non-quenched and tempered steel wire with a diameter of Φ16mm was drawn to Φ13.92mm, and the drawing reduction rate was 24.3%; The first stage of dynamic strain aging is carried out: the drawn wire is heated to 280°C, kept warm for 25 minutes, and then rolled immediately, with the rolling pressure controlled to 0.06mm, and then cold heading is carried out to make the finished bolts; The second stage of dynamic strain aging is to reheat the physical bolts to 150°C, keep them warm for 15 minutes, and then immediately carry out thread rolling, controlling the thread rolling rate to 11r / min.
Citation Information
Patent Citations
Cold forming deformation reinforcement technology during non-tempered steel bolt manufacture process
CN104328261A
Machining method for preventing rolled threads of TC4 titanium alloy material from generating folds
CN105964843A