Heat-resistant flame-retardant decorative paper and preparation method thereof

Through the combination of polyurethane-modified silk fibroin impregnation liquid and gas-phase white carbon black, an IFR system is formed, which solves the problems of flammable and toxic gases in decorative paper, and improves heat resistance and flame retardant performance, ensuring that decorative paper safety and long-term use.

CN116623468BActive Publication Date: 2024-11-05HANGZHOU JINHONG DECORATVE PAPER CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310776352.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-28
Publication Date
2024-11-05
Estimated Expiration
2043-06-28

AI Technical Summary

Technical Problem

Decorative paper is flammable and produces toxic gases during combustion, which poses a fire safety hazard. The existing flame retardant treatment methods use halogen-containing flame retardants to cause harm to human health.

Method used

Polyurethane-modified silk fibroin impregnation liquid is used as the impregnation layer, and the IFR system is formed by introducing phosphate groups, combining gas-phase white carbon black and aqueous starch-based polyurethane prepolymer to form a flame retardant layer, diluting and adsorbing gases generated by combustion , improve the heat resistance and flame retardant properties of decorative paper.

Benefits of technology

It significantly improves the heat-resistant flame retardant and antibacterial properties of decorative paper, reduces the toxic gases generated by combustion, reduces the risk of fire spread, and enhances the service life of decorative paper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004309556870000081
    Figure BDA0004309556870000081
  • Figure BDA0004309556870000091
    Figure BDA0004309556870000091
Patent Text Reader

Abstract

The present application discloses a heat-resistant and flame-retardant decorative paper and a preparation method thereof, wherein the decorative paper comprises base paper, a printing layer, and a dipping layer from the inside to the outside, wherein the dipping layer is formed by dipping the base paper after printing and dipping in a dipping solution, wherein the dipping solution comprises the following raw materials in parts by weight: 120-160 parts of polyurethane-modified silk fibroin dipping solution, and 5-15 parts of a surfactant, wherein the polyurethane-modified silk fibroin dipping solution is obtained by emulsifying a water-based polyurethane prepolymer and a modified silk fibroin after blending, and the modified silk fibroin is obtained by introducing a phosphoric acid group into the silk fibroin. The decorative paper prepared by the present application is green and environmentally friendly, and has good heat resistance, flame retardancy, and antibacterial properties, and can reduce safety hazards and reduce bacterial growth.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of decorative paper, and in particular to a heat-resistant and flame-retardant decorative paper and a preparation method thereof. Background Art

[0002] Decorative paper is a commonly used building material, which is often applied to the surface of boards to provide decorative patterns and cover to prevent the bottom glue from seeping through.

[0003] However, compared with board materials, decorative paper has a higher volatile matter and is extremely flammable, so it can easily become a source of fire, which may further cause the combustion of board materials and cause a fire indoors, posing certain safety hazards.

[0004] At present, the flame retardant treatment of decorative paper on the market generally involves adding halogen-containing flame retardants. However, during the combustion process, decorative paper with halogen-containing flame retardants added will produce toxic gases, which are harmful to human health. Summary of the invention

[0005] In order to improve the heat-resistant and flame-retardant properties of decorative paper and reduce the toxic gases generated by combustion, the present application provides a heat-resistant and flame-retardant decorative paper and a preparation method thereof.

[0006] In a first aspect, a heat-resistant and flame-retardant decorative paper comprises, from the inside to the outside, a base paper, a printing layer, and an impregnation layer, wherein the impregnation layer is formed by impregnating the base paper with an impregnation solution after printing, wherein the impregnation solution comprises the following raw materials in parts by weight: 120-160 parts of a polyurethane-modified silk fibroin impregnation solution and 5-15 parts of a surfactant, wherein the polyurethane-modified silk fibroin impregnation solution is obtained by emulsifying a mixture of an aqueous polyurethane prepolymer and a modified silk fibroin, and wherein the modified silk fibroin is obtained by introducing a phosphate group into the silk fibroin.

[0007] Typically, but not limiting, the surfactant used is sodium dodecylbenzene sulfonate.

[0008] By adopting the above technical solution, silk fibroin is a high molecular fiber protein with good film-forming properties, surface activity, biocompatibility and certain adhesion. After blending with polyurethane, it can improve the adhesion and mechanical properties of the impregnating liquid and give the impregnating liquid a certain repair ability, thereby improving the adhesion effect and action time of the impregnating liquid and further improving the heat resistance of the decorative paper.

[0009] In addition, silk fibroin contains a large amount of amino groups, which can produce a large amount of inert gases such as ammonia and nitrogen when heated, thereby diluting the combustible gas produced by the thermal decomposition of polyurethane. Silk fibroin can also absorb the toxic gas produced when polyurethane burns, achieving the effect of smoke suppression and flame retardancy.

[0010] When phosphate groups are introduced into silk fibroin, the entire polyurethane-modified silk fibroin forms an IFR system. Combustion will produce metaphosphoric acid or polymetaphosphoric acid as an acid source, and the polyurethane with a large number of carbon chains will be used as the carbon source in the IFR system. When silk fibroin is used as the gas source, the originally flammable polyurethane will char and expand during combustion to form a non-flammable carbonized thin layer with a hierarchical structure, and the layers are filled with inert gas, which reduces heat conduction while covering the unburned substrate and reducing the spread of combustion, thereby greatly improving the flame retardant ability of the decorative paper.

[0011] Preferably, the modified silk fibroin comprises the following components in parts by weight: 24-30 parts of silk fibroin, 2-3 parts of polyhexamethylene guanidine phosphate, and 1-2 parts of a catalyst.

[0012] Typically, but not limiting, the catalyst is selected from one of N,N'-diisopropylcarbodiimide, dicyclohexylcarbodiimide and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide.

[0013] By adopting the above technical scheme, there are a large number of amino groups on the silk fibroin. Through the action of the catalyst, the silk fibroin and the polyhexamethylene guanidine phosphate undergo an amidation reaction to complete the grafting of the polyhexamethylene guanidine phosphate on the silk fibroin; the phosphate group is introduced to form an IFR system with the silk fibroin and the polyurethane, thereby improving the flame retardancy of the decorative paper; the polyhexamethylene guanidine phosphate has a certain structure-maintaining ability for the silk fibroin, which can reduce the deconstruction of the β structure of the silk fibroin due to the solubility in water and the binding effect with the polyurethane molecular chain, and reduce the agglomeration effect of the silk fibroin, thereby improving the dispersibility of the polyurethane-modified silk fibroin impregnation solution, and then improving the heat resistance and flame retardancy of the polyurethane-modified silk fibroin impregnation solution; in addition, the polyhexamethylene guanidine phosphate has a large number of guanidine groups, which can adsorb various bacteria and destroy their cell membranes, thereby achieving a bactericidal effect, and the polyurethane has a certain anti-fungal ability. The synergistic effect of the polyurethane and the polyhexamethylene guanidine phosphate can significantly improve the antibacterial ability of the decorative paper, thereby improving the service life of the decorative paper.

[0014] Preferably, the waterborne polyurethane prepolymer comprises the following components by weight: 24-30 parts of polyol, 8-12 parts of isocyanate, 1-2 parts of hydrophilic chain extender, 0.8-1.2 parts of chain extender, 0.01-0.03 parts of catalyst and 24-30 parts of acetone, wherein the polyol is acetylated starch.

[0015] Typically, but not limiting, the acetylated starch is acetylated distarch adipate.

[0016] By adopting the above technical scheme, starch is selected as the polyol to form an aqueous starch-based polyurethane prepolymer, which has the characteristics of high residual carbon content and low decomposition temperature. It can form carbon in advance when the high molecular polymer is thermally decomposed, thereby improving the flame retardant properties of heat-resistant flame-retardant decorative paper; in addition, when used in combination with modified silk fibroin, the flame retardant effect of the formed IFR system is better. In addition, the aqueous starch-based polyurethane prepolymer has good hydrophilicity, which can improve the poor hydrophilicity of modified silk fibroin, thereby affecting the wettability of the polyurethane-modified silk fibroin impregnation solution, and further improve the dispersion performance of the impregnation solution, thereby improving the heat resistance and adhesion effect of the decorative paper.

[0017] Preferably, the polyurethane-modified silk fibroin impregnation solution comprises the following components in parts by weight: 80-86 parts of aqueous polyurethane prepolymer, 14-20 parts of modified silk fibroin and 50-62 parts of deionized water.

[0018] By adopting the above technical scheme, the components of the polyurethane-modified silk fibroin impregnation solution are optimized, the wettability and hydrophobicity of the polyurethane-modified silk fibroin impregnation solution are balanced, the antibacterial ability of the decorative paper is improved while the adhesion performance of the decorative paper is improved, and the flame retardant effect of the IFR system is further improved, thereby significantly improving the heat resistance, flame retardant and antibacterial properties of the decorative paper.

[0019] Preferably, the raw materials of the polyurethane-modified silk fibroin impregnation solution also include fumed silica, and the weight ratio of the fumed silica to the modified silk fibroin is (1-2):(14-20).

[0020] By adopting the above technical scheme, fumed silica, as a non-combustible inorganic substance, can play a certain flame retardant role on the surface of decorative paper; in addition, fumed silica has a large specific surface area and more surface charge, and can adsorb the carbon layer during combustion, thereby increasing the thickness of the single carbon layer; and forming a porous structure on the carbon layer, so that the carbon layers are further filled with inert gas, reducing the heat energy passing through the impregnation layer and transferring to the paper, protecting the paper from thermal decomposition, and fumed silica can also adsorb the smoke generated by the combustion of the substrate, thereby achieving the effects of heat insulation, smoke suppression and flame retardancy, and further improving the heat resistance and flame retardancy of the decorative paper.

[0021] At the same time, the silicon element in fumed silica will reduce the surface energy of the decorative paper, thereby improving the hydrophobicity of the interface between the decorative paper and the outside world, reducing bacterial growth, and thus reducing the damage of microorganisms to the impregnation layer, thereby improving the heat resistance, flame retardancy and antibacterial properties of the decorative paper.

[0022] In a second aspect, a method for preparing heat-resistant and flame-retardant decorative paper is provided, which is prepared by the following steps:

[0023] The printed base paper is coated with a surfactant, and then immersed in a polyurethane-modified silk fibroin impregnation solution, and then taken out and dried at 70-85° C. to obtain heat-resistant and flame-retardant decorative paper.

[0024] Preferably, the amount of glue applied during dipping is 30 g / m 2 .

[0025] By adopting the above technical solution, first coating the surfactant and then impregnating, the dispersibility of the polyurethane-modified silk protein impregnation liquid can be improved, thereby improving the heat resistance and flame retardancy of the decorative paper. After impregnation, the silk protein is taken out and dried at a temperature of 70-85°C, which can reduce the decomposition of the starch base while making the crystal structure of the silk protein change from the β-folding state to the SilkI structure. The silk protein has a certain hydrophilicity under this structure, and its peptide chain is arranged in an antiparallel β-folding structure. More active groups are exposed on the surface of the peptide chain, which can form more hydrogen bonds with the polyurethane, improve the ductility and stability of the impregnation liquid, and further improve the heat resistance of the decorative paper. In addition, with the increase of the use time, the SilkI structure of the silk protein will be further transformed into a more stable SilkII structure. The silk protein under this structure is more hydrophobic and heat-resistant, and further synergistic with fumed silica and polyhexamethylene guanidine phosphate to improve the antibacterial effect and achieve long-term heat resistance and flame retardancy.

[0026] In summary, this application has the following beneficial effects:

[0027] 1. A polyurethane-modified silk fibroin impregnation solution is prepared by blending water-based starch-based polyurethane prepolymer, modified silk fibroin and fumed silica, and the water-based polyurethane prepolymer is used as a carbon source, and the modified silk fibroin with a phosphate group is used as a gas source and an acid source to form an IFR system with good flame retardant effect, and has a good adsorption effect on smoke, thereby improving the flame retardant effect of decorative paper.

[0028] 2. Polyhexamethylene guanidine phosphate is selected as the raw material for modified silk fibroin. Polyhexamethylene guanidine phosphate has good antibacterial properties and can synergize with water-based starch-based polyurethane to further improve the antibacterial properties of decorative paper. In addition, when the dosage of polyhexamethylene guanidine phosphate is optimized, polyhexamethylene guanidine phosphate has a certain stabilizing effect on the structure of silk fibroin, which can reduce the destruction of the spatial structure of silk fibroin after it is dissolved in the solvent and mixed with polyurethane, thereby improving the heat stability and flame retardant properties of the polyurethane-modified silk fibroin impregnation solution.

[0029] 3. By optimizing the preparation process conditions, the compatibility between modified silk fibroin and polyurethane is improved during the polyurethane-modified silk fibroin impregnation process, thereby improving the effect of the polyurethane-modified silk fibroin impregnation. And as the use time increases, through the transformation of the modified silk fibroin structure, the modified silk fibroin can synergize with fumed silica to improve the hydrophobicity of the surface of the decorative paper in contact with the outside world, thereby improving the long-term heat resistance, flame retardancy and antibacterial properties of the decorative paper. DETAILED DESCRIPTION

[0030] The raw materials used in the examples and preparation examples are all commercially available and described in detail. The present application is further described in detail below in conjunction with the examples.

[0031] Preparation of modified silk fibroin

[0032] Preparation Example 1-1, a modified silk fibroin, prepared by the following steps:

[0033] Take 27g of silk fibroin and dissolve it in 500mL of 30% ethanol solution, add 1.5g of N,N′-diisopropylcarbodiimide and react for 40min, then add 2.5g of polyhexamethyleneguanidine phosphate, mix and react for 30h, filter, wash and dry to obtain modified silk fibroin.

[0034] Preparation Example 1-2, a modified silk fibroin, prepared by the following steps:

[0035] 30 g of silk fibroin was dissolved in 500 mL of 30% ethanol solution, 2 g of N, N′-diisopropylcarbodiimide was added and reacted for 60 min, then 3 g of polyhexamethyleneguanidine phosphate was added and mixed for 36 h, filtered, washed and dried to obtain modified silk fibroin.

[0036] Preparation Example 1-3, a modified silk fibroin, is prepared by the following steps:

[0037] Take 24g of silk fibroin and dissolve it in 500mL of 30% ethanol solution, add 1g of N,N′-diisopropylcarbodiimide and react for 60min, then add 2g of polyhexamethyleneguanidine phosphate, mix and react for 24h, filter, wash and dry to obtain modified silk fibroin.

[0038] Preparation Example 1-4, a modified silk fibroin, is different from Preparation Example 1-1 in that the amount of polyhexamethylene guanidine phosphate added is 6 g.

[0039] Preparation Example 1-5, a modified silk fibroin, is different from Preparation Example 1-1 in that the amount of polyhexamethyleneguanidine phosphate added is 0.5 g.

[0040] Preparation Example 1-6, a modified silk fibroin, is different from Preparation Example 1-1 in that polyhexamethyleneguanidine phosphate is replaced by an equal amount of ammonium polyphosphate.

[0041] Preparation of waterborne polyurethane prepolymer

[0042] Preparation Example 2-1, a waterborne polyurethane prepolymer is prepared by the following steps:

[0043] Prepolymerization: 27 g of acetylated distarch adipate was dissolved in 200 mL of N,N-dimethylformamide, and then 10 g of isophorone diisocyanate and 0.02 g of dibutyltin laurate were added and mixed, and the mixture was reacted for 2 h to obtain a prepolymer;

[0044] Chain extension reaction: 1.5 g 1,4-butanediol, 1 g diethyltoluenediamine and 27 g acetone were added to the prepolymer and reacted for 2 h to obtain a waterborne polyurethane prepolymer.

[0045] Preparation Example 2-2, a waterborne polyurethane prepolymer is prepared by the following steps:

[0046] Prepolymerization: 30 g of acetylated distarch adipate was dissolved in 200 mL of N,N-dimethylformamide, and then 12 g of isophorone diisocyanate and 0.03 g of dibutyltin laurate were added and mixed, and the mixture was reacted for 2.5 h to obtain a prepolymer;

[0047] Chain extension reaction: 1 g of 1,4-butanediol, 1.2 g of diethyltoluenediamine and 30 g of acetone were added to the prepolymer and reacted for 3 h to obtain a waterborne polyurethane prepolymer.

[0048] Preparation Example 2-3, a waterborne polyurethane prepolymer is prepared by the following steps:

[0049] Prepolymerization: 24 g of acetylated distarch adipate was dissolved in 200 mL of N,N-dimethylformamide, and then 8 g of isophorone diisocyanate and 0.01 g of dibutyltin laurate were added and mixed, and the mixture was reacted for 1.5 h to obtain a prepolymer;

[0050] Chain extension reaction: 2 g of 1,4-butanediol, 0.8 g of diethyltoluenediamine and 24 g of acetone were added to the prepolymer and reacted for 1 h to obtain a waterborne polyurethane prepolymer.

[0051] Preparation Example 2-4, a waterborne polyurethane prepolymer, is different from Preparation Example 2-1 in that acetylated distarch adipate is replaced by an equal amount of poly(1,6-hexanediol adipate).

[0052] Preparation of polyurethane-modified silk fibroin

[0053] Preparation Example 3-1, a polyurethane-modified silk fibroin impregnation solution, is prepared by the following steps:

[0054] 17 g of modified silk fibroin was dissolved in 200 mL of acetone solution, 83 g of aqueous polyurethane prepolymer and 1.5 g of fumed silica were added and mixed evenly, allowed to stand for 12 h, and then 56 g of deionized water was added for emulsification, and the acetone was removed by suction to obtain a polyurethane-modified silk fibroin impregnation solution.

[0055] Wherein, the modified silk fibroin is derived from Preparation Example 1-1, and the waterborne polyurethane prepolymer is derived from Preparation Example 2-1.

[0056] Preparation Example 3-2, a polyurethane-modified silk fibroin impregnation solution, is prepared by the following steps:

[0057] 20 g of modified silk fibroin was dissolved in 200 mL of acetone solution, 80 g of aqueous polyurethane prepolymer and 1 g of fumed silica were added and mixed evenly, and the mixture was allowed to stand for 14 h. Then, 50 g of deionized water was added for emulsification, and the acetone was removed by suction to obtain a polyurethane-modified silk fibroin impregnation solution.

[0058] Wherein, the modified silk fibroin is derived from Preparation Example 1-2, and the waterborne polyurethane prepolymer is derived from Preparation Example 2-2.

[0059] Preparation Example 3-3, a polyurethane-modified silk fibroin impregnation solution, is prepared by the following steps:

[0060] 14 g of modified silk fibroin was dissolved in 200 mL of acetone solution, 86 g of aqueous polyurethane prepolymer and 2 g of fumed silica were added and mixed evenly, and the mixture was allowed to stand for 10 h. Then 62 g of deionized water was added for emulsification, and the acetone was removed by suction to obtain a polyurethane-modified silk fibroin impregnation solution.

[0061] Wherein, the modified silk fibroin is derived from Preparation Example 1-3, and the waterborne polyurethane prepolymer is derived from Preparation Example 2-3.

[0062] Preparation Example 3-4, a polyurethane-modified silk fibroin impregnation solution, is different from Preparation Example 3-1 in that the modified silk fibroin is derived from Preparation Example 1-4.

[0063] Preparation Example 3-5, a polyurethane-modified silk fibroin impregnation solution, is different from Preparation Example 3-1 in that the modified silk fibroin is derived from Preparation Example 1-5.

[0064] Preparation Example 3-6, a polyurethane-modified silk fibroin impregnation solution, is different from Preparation Example 3-1 in that the modified silk fibroin is derived from Preparation Example 1-6.

[0065] Preparation Example 3-7, a polyurethane-modified silk fibroin impregnation solution, is different from Preparation Example 3-1 in that the aqueous polyurethane prepolymer is derived from Preparation Example 2-4.

[0066] Preparation Example 3-8, a polyurethane-modified silk fibroin impregnation solution, is different from Preparation Example 3-1 in that the modified silk fibroin is replaced by an equal amount of unmodified silk fibroin.

[0067] Preparation Example 3-9, a polyurethane-modified silk fibroin impregnation solution, is different from Preparation Example 3-1 in that the fumed silica is replaced by an equal amount of nano-titanium dioxide.

[0068] Example

[0069] Example 1, a heat-resistant and flame-retardant decorative paper, is prepared by the following steps:

[0070] The printed base paper was coated with 10 kg of sodium dodecylbenzene sulfonate, and then immersed in 140 kg of polyurethane-modified silk fibroin impregnation solution for 1.5 hours, taken out, and dried at 78° C. for 3 hours to obtain heat-resistant and flame-retardant decorative paper.

[0071] The polyurethane-modified silk protein impregnation liquid is from Preparation Example 3-1, and the amount of impregnation glue is 30 g / m 2 .

[0072] Embodiment 2, a heat-resistant and flame-retardant decorative paper is prepared by the following steps:

[0073] The printed base paper was coated with 15 kg of sodium dodecylbenzene sulfonate, and then immersed in 160 kg of polyurethane-modified silk fibroin impregnation solution for 2 hours, taken out, and dried at 85° C. for 2 hours to obtain heat-resistant and flame-retardant decorative paper.

[0074] The polyurethane-modified silk protein impregnation liquid is from Preparation Example 3-2, and the amount of impregnation glue is 30 g / m 2 .

[0075] Embodiment 3, a heat-resistant and flame-retardant decorative paper is prepared by the following steps:

[0076] The printed base paper was coated with 5 kg of sodium dodecylbenzene sulfonate, and then immersed in 120 kg of polyurethane-modified silk fibroin impregnation solution for 1 hour, taken out, and dried at 70° C. for 4 hours to obtain heat-resistant and flame-retardant decorative paper.

[0077] The polyurethane-modified silk protein impregnation liquid is from Preparation Example 3-3, and the amount of impregnation glue is 30 g / m 2 .

[0078] Example 4, a heat-resistant and flame-retardant decorative paper, is different from Example 1 in that the polyurethane-modified silk fibroin impregnation liquid is derived from Preparation Example 3-4.

[0079] Example 5, a heat-resistant and flame-retardant decorative paper, is different from Example 1 in that the polyurethane-modified silk fibroin impregnation liquid is derived from Preparation Examples 3-5.

[0080] Example 6, a heat-resistant and flame-retardant decorative paper, is different from Example 1 in that the polyurethane-modified silk fibroin impregnation liquid is derived from Preparation Examples 3-6.

[0081] Example 7, a heat-resistant and flame-retardant decorative paper, is different from Example 1 in that the polyurethane-modified silk fibroin impregnation liquid is derived from Preparation Examples 3-7.

[0082] Embodiment 8, a heat-resistant and flame-retardant decorative paper, is prepared by the following steps:

[0083] Take the printed base paper, coat it with 10 kg of sodium dodecylbenzene sulfonate, and then immerse it in 140 kg of polyurethane-modified silk fibroin impregnation solution, and take it out to obtain heat-resistant and flame-retardant decorative paper (that is, without drying operation).

[0084] The polyurethane-modified silk protein impregnation liquid is from Preparation Example 3-1, and the amount of impregnation glue is 30 g / m 2 .

[0085] Example 9, a heat-resistant and flame-retardant decorative paper, is different from Example 1 in that the polyurethane-modified silk fibroin impregnation liquid is derived from Preparation Examples 3-9.

[0086] Comparative Example

[0087] Comparative Example 1 is a heat-resistant and flame-retardant decorative paper, which is different from Example 1 in that the polyurethane-modified silk fibroin impregnation liquid is derived from Preparation Examples 3-8.

[0088] Comparative Example 2 is a heat-resistant and flame-retardant decorative paper, which is different from Example 1 in that sodium dodecylbenzene sulfonate is replaced by an equal amount of deionized water.

[0089] Comparative Example 3, a heat-resistant and flame-retardant decorative paper, comprising the following steps:

[0090] S1: printing the base paper and drying it at 110°C for 3h to obtain a semi-finished product;

[0091] S2: 80 kg of melamine, 4 kg of amino silicone emulsifier, 2 kg of polyether diamine, 3 kg of mannitol, 1 kg of activated carbon, and 1 kg of release agent were mixed and stirred for 40 min, and then 2 kg of dicyclohexyl aluminum phosphinate, 0.2 kg of magnesium hydroxide, 0.2 kg of aluminum hydroxide and 0.1 kg of pentaerythritol were added, and stirring was continued for 25 min to obtain an impregnation composition;

[0092] S3: The impregnation composition is heated to 120°C, and the semi-finished product is placed in the impregnation composition for the first impregnation and gluing for 1.5 hours, and then the semi-finished product is taken out and dried at 100°C for 30 minutes, and then placed in the impregnation composition again for the second impregnation and gluing for 1.5 hours, and then the semi-finished product is taken out and dried at 110°C for 50 minutes to obtain decorative paper.

[0093] Among them, the first dipping glue coating amount is 30g / m 2 The second dipping amount is 60g / m 2 .

[0094] Performance testing

[0095] The decorative papers of Examples 1-9 and Comparative Examples 1-3 were subjected to performance tests. Each test was conducted 6 times in parallel and the average value was taken. The results are shown in Table 1.

[0096] Test 1: Flame retardancy: The flame retardancy of decorative paper was tested in accordance with GB / T2406.2-2009 “Determination of combustion behavior by oxygen index method Part 2: Room temperature test”.

[0097] Test 2: Thermal stability: The thermal stability of the decorative paper was measured according to CAN ULC-S135 “Heat Release Rate Test”.

[0098] Test 3: Antibacterial property: The decorative papers of Examples 1-7 and Comparative Examples 1-3 were sterilized in a 100°C vacuum oven for 1 hour, and then placed in air for 24 hours and 72 hours. The total number of colonies was determined according to the industry standard YC171-2009 "Cigarette Tipping Paper".

[0099] Table 1: Performance test results of Examples 1-7 and Comparative Examples 1-3

[0100]

[0101]

[0102] It can be seen from Examples 1-9, Comparative Example 3 and Table 1 that the decorative paper prepared in the present application has good heat resistance, flame retardant properties and antibacterial properties. The reason is that the silk fibroin in the modified silk fibroin acts as a gas source and the polyhexamethylene guanidine phosphate in the modified silk fibroin acts as an acid source to convert the originally flammable water-based polyurethane prepolymer into a carbon source to form an IFR system, so that the decorative paper obtains good flame retardant properties and heat resistance after impregnation; in addition, there is also a flame retardant compatibility effect between the fumed silica, the modified silk fibroin and the water-based polyurethane prepolymer, which further improves the flame retardant properties of the decorative paper.

[0103] The polyhexamethylene guanidine phosphate in the modified silk fibroin can work synergistically with the waterborne polyurethane prepolymer to improve the antibacterial properties of the decorative paper.

[0104] At the same time, fumed silica is introduced into the impregnation liquid. The fumed silica and the IFR system have flame retardant and heat-resistant compatibility. The fumed silica and modified silk fibroin can further improve the water repellency of the contact surface between the decorative paper and the external surface, reduce the bacterial growth caused by moisture and the damage to the impregnation layer, so that the decorative paper has long-lasting antibacterial, heat-resistant and flame-retardant properties.

[0105] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A heat-resistant and flame-retardant decorative paper, It is characterized in that The heat-resistant and flame-retardant decorative paper comprises base paper, a printing layer, and a dipping layer from the inside to the outside. The heat-resistant and flame-retardant decorative paper is prepared by the following steps: Taking the printed base paper, coating it with a surfactant, and then dipping it in a polyurethane-modified silk fibroin impregnation solution, taking it out and drying it at 70-85° C. to obtain heat-resistant and flame-retardant decorative paper; The weight portion of the polyurethane-modified silk fibroin impregnation solution is 120-160 parts, and the weight portion of the surfactant is 5-15 parts; The polyurethane-modified silk fibroin impregnation liquid is obtained by emulsifying a waterborne polyurethane prepolymer and a modified silk fibroin after blending; the modified silk fibroin is obtained by introducing a phosphate group into the silk fibroin; The polyurethane-modified silk fibroin impregnation solution comprises the following components in parts by weight: 80-86 parts of waterborne polyurethane prepolymer, 14-20 parts of modified silk fibroin and 50-62 parts of deionized water; The modified silk fibroin comprises the following components in parts by weight: 24-30 parts of silk fibroin, 2-3 parts of polyhexamethylene guanidine phosphate, and 1-2 parts of a catalyst; the catalyst is selected from one of N, N'-diisopropylcarbodiimide, dicyclohexylcarbodiimide and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide; The modified silk fibroin is prepared by the following steps: The silk fibroin is dissolved in an organic solvent, a catalyst is added and stirred, polyhexamethylene guanidine phosphate is added, mixed and reacted, filtered, washed and dried to obtain the modified silk fibroin.

2. The heat-resistant and flame-retardant decorative paper according to claim 1, It is characterized in that The waterborne polyurethane prepolymer comprises the following components in parts by weight: 24-30 parts of polyol, 8-12 parts of isocyanate, 1-2 parts of 1,4-butanediol, 0.8-1.2 parts of diethyltoluenediamine, 0.01-0.03 parts of catalyst and 24-30 parts of acetone.

3. The heat-resistant and flame-retardant decorative paper according to claim 2, It is characterized in that The polyol is acetylated starch.

4. The heat-resistant and flame-retardant decorative paper according to claim 3, It is characterized in that The waterborne polyurethane prepolymer is prepared by the following steps: Prepolymerization: dissolving acetylated starch in an organic solvent, adding isocyanate and a catalyst, and reacting to obtain a prepolymer; Chain extension reaction: 1,4-butanediol, diethyltoluenediamine and acetone are added to the prepolymer to react to obtain a waterborne polyurethane prepolymer.

5. The heat-resistant and flame-retardant decorative paper according to claim 1, It is characterized in that The raw materials of the polyurethane-modified silk fibroin impregnation solution also include fumed silica, and the weight ratio of the fumed silica to the modified silk fibroin is (1-2):(14-20).

6. The heat-resistant and flame-retardant decorative paper according to claim 1, It is characterized in that The preparation method of the polyurethane-modified silk fibroin impregnation solution adopts the following steps: The modified silk fibroin is dissolved in an organic solvent, mixed evenly, and then an aqueous polyurethane prepolymer and fumed silica are added and blended, and then allowed to stand, deionized water is added for emulsification, and the organic solvent is removed by suction to obtain a polyurethane-modified silk fibroin impregnation solution.

Citation Information

Patent Citations

  • Preparation method for hydrolyzed silk protein paint

    CN103146297A

  • Environment-friendly heat-resistant waterborne polyurethane coating

    CN104293159A

  • Anti-flaming anti-peeling polyurethane adhesive

    CN107502275A

  • Heat-resistant flame-retardant decorative paper and preparation method thereof

    CN114032706A

  • Composition for flame retardation, sheet for flame retardation and flame-retardant decorative sheet